Mathieu
Fuentes-Exposito
a,
Sébastien
Norsic
a,
Thibaut
Février
a,
Pierre-Yves
Dugas
a,
Salima
Boutti
b,
Samuel
Devisme
c,
Anthony
Bonnet
b,
Franck
D'Agosto
*a and
Muriel
Lansalot
*a
aUniv Lyon, Université Claude Bernard Lyon 1, CPE Lyon, CNRS, UMR 5128, Catalysis, Polymerization, Processes and Materials (CP2M), 43 Bd du 11 Novembre 1918, 69616 Villeurbanne, France. E-mail: franck.dagosto@univ-lyon1.fr; muriel.lansalot@univ-lyon1.fr
bARKEMA, Centre de Recherche Rhône-Alpes (CRRA), Rue Henri Moissan - CS 42063, 69491 Pierre-Bénite Cedex, France
cARKEMA, Centre de recherche, développement, applications et technique de l'ouest (Cerdato), 13 route de Launay, 27470 Serquigny, France
First published on 13th September 2021
A robust and straightforward synthesis of surfactant-free poly(vinylidene fluoride) (PVDF) latexes is presented using RAFT/MADIX-mediated emulsion polymerization. VDF emulsion polymerizations were conducted in the presence of commercial poly(ethylene glycol) chains (PEG-OH) and in the presence of the same chains carrying a dithiocarbonate (xanthate) chain end (PEG-X). The identification of the stabilization mode in both cases is carefully examined, considering the irreversible chain transfer reactions well known in VDF free radical polymerization. The particle size is significantly smaller when PEG-X was used, demonstrating the positive effect on particle stabilization of the involvement of xanthate chain end in the free radical process.
To address the constraints related to the use of fluorinated and low molar surfactants, various poly(ethylene glycol) (PEG) based-molecules have been used and depicted in the patent literature related to VDF emulsion polymerization, however mainly for the synthesis of poly(vinylidene fluoride-co-hexafluoropropylene).21–25 Surfactant-free PVDF-based latexes were thus obtained using reactive PEG (meth)acrylate macromonomers. Surprisingly, unreactive hydrosoluble PEG-OH chains alone can also act as precursor of stabilizer during the emulsion polymerization process by providing stable latexes. The patent literature mentioned above does however not provide any mechanistic details on how commercial PEG-OH can bring particle stability. Nevertheless, VDF free radical polymerization is known to be prone to chain transfer reactions to the monomer, to the polymer (via inter- (long chain branching) or intramolecular (short chain branching) transfer reaction) and to chain transfer agents such as e.g. ethyl acetate.4,5,7,26 Indeed, labile hydrogen atoms carried by these species could be abstracted by the very reactive PVDF propagating macroradicals leading to new radicals, which should initiate new PVDF polymer chains. In that context, chain transfer reactions occurring along PEG-OH chains during the emulsion (co)polymerization of VDF could thus form short PVDF grafts along the PEG chains and result in the in situ formation of an amphiphilic stabilizer.
The advances achieved in polymer synthesis by reversible-deactivation radical polymerization (RDRP) techniques over the last 20 years have pushed forward the use of living hydrophilic polymers for the synthesis of polymer particles in emulsion. Indeed, these well-defined and reactive macromolecules can be chain-extended with a hydrophobic monomer directly in water leading to the in situ formation of amphiphilic block copolymers that simultaneously self-assemble into polymer nanoparticles. The process, coined polymerization-induced self-assembly (PISA), can be applied to different polymerization techniques,27–30 but the most studied one undoubtedly remains reversible addition–fragmentation chain transfer (RAFT)/macromolecular design by interchange of xanthates (MADIX).31,32 PISA is also applicable in dispersion polymerization (where the core forming monomer is soluble in the continuous phase), both in aqueous and organic media.31,33–35 Hence, water-soluble chains obtained either by the RAFT polymerization of hydrophilic monomers or via the chemical modification of preformed polymers can act as chain transfer agent (and referred to as macroCTA) generating stabilizers during an emulsion polymerization by forming amphiphilic block copolymers in situ. PEG-based macroCTA have thus been reported for the PISA synthesis of various kinds of particles,36–51 but to the best of our knowledge, never for PVDF latexes.
Using very low amounts of such macroCTA in an emulsion polymerization seems to be an economically viable approach to access surfactant-free latexes. In that case, the initial amount of the macroCTA is such that enough amphiphilic block copolymers are formed in situ to ensure stabilization of the particles produced simultaneously by emulsion polymerization. This approach is actually quite interesting for the synthesis of industrially relevant polymer latexes, for instance in paint technology, where the fraction of hydrophilic species in the final coating must remain low. Using this strategy, we indeed prepared high solids content (ca. 40 wt%) polymer latexes incorporating less than 2 wt% of hydrophilic species with poly(vinylidene chloride)52,53 and polyacrylics.54–57 The stabilizer being strongly anchored to the particle surface at the end of the emulsion polymerization, the obtained latexes led to polymer films with enhanced water barrier properties. The strategy was also successful for the synthesis of poly(vinyl acetate-co-ethylene).58
In the present paper, emulsion polymerization of VDF is conducted for the first time in the presence of hydrophilic RAFT/MADIX macroCTA. In order to accurately comprehend the role of the thiothiocarbonylated chain end in the process, PEG-OH chains and their analogues equipped with a dithiocarbonate (xanthate) moiety (PEG-X) have been comparatively evaluated in the synthesis of surfactant-free synthesis of PVDF latexes. Several parameters are varied such as the PEG molar mass and the macroCTA structure (mono versus bifunctional xanthate) (Scheme 1).
1H NMR (400 MHz, CDCl3, δ): 4.6 (q, 2H, O–CH2–CH3); 4.4 (q, 1H, CH–S); 4.3 (t, 2H, CH2–CH2–O); 3.75–3.5 (s, 180H, (CH2–CH2–O)n); 3.35 (s, 3H, CH3–O); 1.6 (d, 3H, CHCH3); 1.4 (t, 3H, CH2–CH3).
The same procedure was followed with another commercial PEG-OH (Mn = 750 g mol−1), leading to PEG-X with Mn,SEC = 1300 g mol−1 and Đ = 1.10. The 1H NMR spectrum of the final product is shown in Fig. S3,† while Fig. S4† displays the chromatogram obtained by SEC analyses in THF using PS standards.
1H NMR (400 MHz, (CD3)2CO, δ): 4.6 (q, 2H, O–CH2–CH3); 4.4 (q, 1H, CH–S); 4.3 (t, 2H, CH2–CH2–O); 3.8–3.5 (s, 70H, (CH2–CH2–O)n); 3.3 (s, 3H, CH3–O); 1.55 (d, 3H, CH–CH3); 1.4 (t, 3H, CH2–CH3).
1H NMR (400 MHz, CDCl3, δ): 4.6 (q, 2H, O–CH2–CH3); 4.4 (q, 1H, CH–S); 4.3 (t, 2H, CH2–CH2–O); 3.75–3.5 (s, 220H, (CH2–CH2–O)n); 1.6 (d, 3H, CHCH3); 1.4 (t, 3H, CH2–CH3).
For a scale-up experiment, VDF emulsion polymerization was carried out in a 4 L high pressure stainless steel autoclave equipped with a nitrogen inlet, a thermometer, a mechanical stirrer and a pressure sensor. The reactor temperature was measured by a thermocouple J Atex, protected by a metal tube and placed inside the reactor. Oil (Ultra 350, Lauda) circulating in the jacket was used to control the reactor temperature (no oil circulated in the cover neither the bottom). The inlet and outlet temperature of the circulating oil in the reactor jacket was measured with a platinum resistance Pt100. The reactor pressure was monitored with a pressure sensor Atex (type PA-23EB, Keller). In a typical polymerization procedure, KPS, PEG-OH (or PEG-X), buffer (sodium acetate) and deionized water (2 L) were introduced in the reactor. The medium was deoxygenated under nitrogen for 30 min. VDF gas was fed into the reactor until the targeted pressure (30 bar). Immediately after, the injection port was closed and the medium heated at a set point temperature of 80 °C. When the temperature inside the reactor dropped below 25 °C, the remaining pressure was carefully released, and the obtained latex was collected, and the particle size was measured. A fraction of the obtained latex was dried for SC measurement, which after subtraction of nonpolymeric species gave the PC. The dried polymer was then used for polymer characterization by DSC.
Xc(%) = (ΔHf,measured/ΔHf,∞) × 100 |
Exp.a | Stabilizer | KPS/stabilizerb | Time (h) | SCc (%) | PEG fractione (wt%) | D z f (nm) | PdIf | N p (×1016 L−1latex) | |
---|---|---|---|---|---|---|---|---|---|
Name | n | ||||||||
a T = 80 °C; P = 30 bar. Fixed amount of KPS (7.3 mmol L−1) and sodium acetate – Variable PEG nature and weight. n = number of ethylene glycol units. b Weight ratio. c Solids content taking into account all the non-volatile species (including stabilizer and PVDF). d Performed in a 4 L reactor in the presence of 2 L of water, 4 g of KPS, 2.5 g of sodium acetate and 1.6 g of PEG-X or PEG-OH. e Weight fraction of PEG in the final latex considering the initial amount of PEG species and the final amount of PVDF. f Determined by DLS. g The PdI of this sample was high (0.7) and the Dz value was thus not considered as relevant. | |||||||||
L01 | PEG-OH | 44 | 2.5 | 4 | 11.2 | 0.7 | 234 | 0.01 | 0.9 |
L02 | — | — | — | 1 | 7.8 | — | 378 | 0.31 | — |
L03 | PEG-X | 44 | 2.5 | 4 | 10.4 | 0.8 | 72 | 0.06 | 30.3 |
L04 | PEG-SH | 44 | 2.5 | 3.25 | 8.1 | 1.0 | 95 | 0.04 | 10.1 |
L05 | PEG-X | 44 | 1.25 | 8 | 2.4 | 6.7 | —g | —g | — |
L06 | 5 | 4 | 14.4 | 0.3 | 101 | 0.05 | 15.2 | ||
L07 | PEG-X | 15 | 2.5 | 4 | 10.4 | 0.8 | 62 | 0.06 | 47.5 |
L08 | 6.7 | 4 | 15.9 | 0.2 | 99 | 0.03 | 17.9 | ||
L09 | X-PEG-X | 44 | 2.5 | 4 | 8.5 | 0.9 | 72 | 0.06 | 24.1 |
L10d | PEG-OH | 44 | 2.5 | 4.25 | 7.6 | 1.1 | 225 | 0.04 | 0.7 |
L11d | PEG-X | 44 | 2.5 | 4.25 | 6.8 | 1.2 | 72 | 0.06 | 19.5 |
This result was explained by the peculiar reactivity of the propagating radicals in VDF polymerization. Indeed, as mentioned in the introduction and depicted in the literature, irreversible transfer reactions are particularly pronounced in the presence of hydrogenated species. All the hydrogens atoms of PEG-OH are adjacent to the oxygen atoms and thus labile. They are probably responsible for the inhibition observed. These first unsuccessful experiments give an additional information. The inhibition observed is indeed consistent with a degradative chain transfer, i.e. without subsequent efficient reinitiation of the VDF polymerization (Scheme 2A-a). Decreasing the amount of PEG versus KPS would allow, once enough reactive transfer sites on the PEG chains (hydrogen atoms adjacent to the oxygen ones) have been neutralized by forming an amphiphilic structure after coupling (Scheme 2A-b), to produce enough radicals to efficiently start the polymerization. Indeed, L01 provided a stable latex with particle size of 234 nm. The stability of the latex obtained cannot be explained only by the charges provided by the initiator KPS. The latter contribution is indeed real, as attested by the formation of a stable PVDF latex in the sole presence of KPS under the same conditions (Table 1, L02, 7.8 wt% solids after 1 h). However, the large particle size obtained in that case (378 nm) compared to the latex formed in the presence of PEG-OH (L01, 234 nm) indicates a beneficial contribution of this macromolecule on the particle stability. As mentioned above, in L01, the amount of PEG used (20 mg, for a final weight fraction of 0.7 wt% with respect to PVDF, Table 1) makes the isolation and the characterization of the stabilizer formed almost impossible. Taking into account the observed inhibition when the KPS/PEG-OH weight ratio is too low, these structures would not be the result of a reinitiation of the polymerization of VDF on the PEG after a transfer reaction, although this cannot be completely rule out.
Indeed, reinitiation of VDF polymerization by –CH2–CH˙(OMe) has been reported in the literature.59 In this work, the successful synthesis of block copolymers based on poly(methyl vinyl ether) (PMVE) and PVDF segments was achieved by a combination of cationic RAFT and RAFT polymerizations. PMVE chains carrying a dithiocarbamate chain end (PMVE-DTC) were used to control RAFT polymerization of VDF. This however takes place in dimethylcarbonate, a good solvent for VDF, whereas VDF is only slightly soluble in water. In addition, VDF affinity for a hydrophilic polymer such as PEO dissolved in water is low compared to the affinity of VDF for PMVE in DMC. Besides, oligomers of PVDF formed in water in an emulsion process (+K,−OSO3-PVDF˙) will carry an anionic charge (coming from the KPS initiator) and their affinity with hydrosoluble species will be increased favoring both transfer reaction but also coupling reactions with PEG chains. In that case, the bimolecular termination between a growing hydrosoluble +K,−OSO3-PVDF˙ oligoradical and the radical generated by transfer between another growing hydrosoluble +K,−OSO3-PVDF˙ oligoradical and PEG (Scheme 2A-b) will likely be favored. The negative charges carried by−OSO3-PVDF˙ oligomers or by the grafted structure, would favorably contribute to stabilization of the particles.
As mentioned above, the presence of additional PVDF grafts resulting from reinitiation after transfer (thus not carrying sulfate groups) cannot completely be ruled out (Scheme 2B, red PVDF grafts). Eventually, transfer reactions on the hydrogen of the tertiary carbon atom formed by the previous assumed reactions (coupling or reinitiation) are also possible although, considering steric effects, the formation of two grafts on the same carbon may be disfavored (Scheme 2B, green PVDF grafts). Scheme 2B represents a structure in which all the above possibilities are compiled. For the sake of clarity, this structure only accounts for the normal head-to-tail additions of propagating radicals (–CH2CF2–CH2CF2–) onto VDF and not for the well-known and more complicated microstructure of PVDF produced by free radical polymerization, which additionally includes head-to-head (–CH2CF2–CF2CH2–) and tail-to-tail (–CF2CH2–CH2CF2–) additions.1,60
Strong of these first understandings on the potential stabilization mechanisms and on the role of PEG-OH as precursor of stabilizer in VDF emulsion polymerization, we then investigated the use of PEG-X (Mn = 2300 g mol−1 and Đ = 1.03) as stabilizer precursor. The choice of the installation of a xanthate moiety at the end of the PEG chains was dictated by the good control observed when RAFT polymerization of VDF was conducted in organic solvent61–68 and by the successful block copolymer syntheses reported in organic solvent by chain extension using polymers functionalized with xanthate chain ends,69–72 including an attempt to perform VDF PISA in dimethyl carbonate from a poly(vinyl acetate) macroCTA.70 These results were a strong indication that a chain extension of PEG-X with VDF could take place in our systems although it does not exclude the occurrence of the grafting reactions very specific from the emulsion polymerization process and identified above. The commercial PEG-OH used above was chemically modified to introduce the xanthate functionality. The xanthate is meant to promote reversible transfer reactions at the end of the chain and minimize degradative chain transfer reactions along the PEG chain as observed when RDRP of VDF was performed.61,63,73–75 A stable PVDF latex is indeed obtained in presence of PEG-X (Table 1 – L03). After 4 hours of polymerization the solids content (10.4%) is very similar to the one obtained with PEG-OH (11.2%, L01) showing that the presence of the xanthate chain ends does not significantly affect the yield of polymer produced. It is worth mentioning that a comparative kinetic study presented in Fig. S7† shows that the snapshot given after 4 hours of polymerization does not hide a completely different kinetic behaviour between PEG-OH and PEG-X. Indeed, rather similar kinetic profiles were observed, with a different but steady polymerization rate in both cases.
Besides, isometric particles with a size of 72 nm are obtained compared to 234 nm with PEG-OH. This result shows the strong and beneficial impact of favoring chain transfer reaction via the xanthate group on particle stabilization. This goes along with a higher number of formed particles when using PEG-X (almost 30 times higher, see L01 and L03 in Table 1). This is further attested by cryo-TEM pictures of the corresponding PVDF latexes (Fig. 1). The difference in sizes observed with DLS is confirmed by cryo-TEM. Besides, brighter areas corresponding to less electron dense parts are visible by cryo-TEM inside the PVDF particles synthesized with PEG-OH (Fig. 1A). This phenomenon has already been reported for particles synthesized with PEG-based macroCTA,19,76 PEG-based stabilizers77,78 or initiators,79 or even KPS alone.80 These parts probably correspond to the formation of water pockets during the emulsion polymerization, resulting from buried PEG-based species inside the particles and leading to the brighter area observed during cryo-TEM analysis. This corroborates the fact that the structure shown in Scheme 2B is probably not the optimum one to act as stabilizer and to stabilize water/PVDF interfaces. The much smaller size and the absence of less electron dense parts inside the particles when PEG-X is used (Fig. 1C) confirm the superior ability of PEG-X to act as a (precursor of) stabilizer in this case. The formation of a PVDF segment from the chain end of PEG-X, PVDF segment probably longer than the side PVDF grafts as resulting from a reversible transfer from the xanthate chain end, would then drive the anchorage of the overall structure as depicted in Scheme 2C, at the surface of the particles optimizing the stabilization.
Fig. 1 Cryo-TEM images of PVDF particles prepared with (A) PEG-OH (L01), (B) PEG-SH (L04) and (C) PEG-X (L03). |
The beneficial effect of the reversibility of the transfer reaction induced by the xanthate moiety can be supported by experiment L04 in which PEG chains carrying a thiol chain end (PEG-SH – Mn = 2000 g mol−1) were used instead of PEG-X. In this case, a lower yield (solids content 8.1%) was obtained after 3.25 h while the particle size was already larger (95 nm, Fig. 1B) than the one obtained with PEG-X. PEG-SH has been previously used in emulsion polymerization of styrene to generate block copolymers surfactant during the process.14 Besides, thiols are known to induce irreversible chain transfer reactions in VDF polymerization.81 As a result, the small size particles obtained with PEG-SH confirm the formation of short PVDF segments from PEG via irreversible chain transfer and thus in situ formation of stabilizers. It further shows the superiority of the reversible chain transfer reaction induced by the xanthate for the stabilization of PVDF latex.
The above results showed that the presence of xanthate chain end favors reversible chain transfer at the end of PEG chains over the degradative chain transfer reactions along the PEG backbone. In that respect, we hoped to be able to slightly increase the amount of PEG-X in the formulation without lowering too much the final solids content for the same polymerization time. This could have also eased the identification of the chemical modifications occurring on the PEG during the emulsion process. However, when increasing the amount of PEG-X in the recipe (KPS/PEG-X weight ratio of 1.25 in L05, Table 1), the solids content greatly decreased to only 2.4% even after a prolonged polymerization time (8 hours). This phenomenon is directly linked to the increase in the content of hydrogenated species. Indeed, decreasing on the other hand PEG-X content to reach a KPS/PEG-X ratio of 5 (L06) allowed the formation of 100 nm PVDF particles, with a solids content of 14.4% in 4 hours.
As mentioned above, the initial amount of PEG-X cannot allow a classical structural characterization of the PEG chains after polymerization. Indeed, the final weight fraction of PEG (with respect to the formed PVDF) in these latexes is typically lower than 1 wt% (except for the low SC latex L05, Table 1). Nevertheless, the strategy remains very interesting as it minimizes the amount of stabilizer precursor and in the end the fraction of hydrophilic species in the final latexes. Indirect information on the structure of the stabilizer can however be gathered by additional physico-chemical characterizations of the final latex. Surface tension analyses were thus performed on L01 (PVDF latex from PEG-OH) and L03 (PVDF latex from PEG-X) in order to quantify in both systems, the amount of free PEG chains, i.e., not participating to particle stabilization. Calibration curves were first established by measuring the surface tension of aqueous solutions of various concentrations of PEG-OH and PEG-X (Fig. S8†). According to the calibration curve, 82.5 wt% of the initial amount of PEG-OH is present as free chains in the final latex L01, whereas only 1.0 wt% of the initial amount of PEG-X is present as free polymer chains in the latex L03. These very contrasted results are fully consistent with the superiority of PEG-X compared to PEG-OH to stabilize PVDF latex obtained by emulsion polymerization. As a comparison, using the same surface tension measurements, 23 wt% of the initial PEG-SH was present as free chains, results consistent with a lower efficacity of stabilization in this case, as discussed above. All these data should however be considered with care as the surface tension measured may not be only the reflect of the contribution of free PEG chains in the water phase. Indeed, the aqueous phase may also contain grafted fluorinated PEG species (see Scheme 2), the contribution of which will not be accurately reflected by the calibration curves obtained from the initial PEG species (i.e., PEG-OH, PEG-X or PEG-SH).
The VDF emulsion polymerizations conducted with PEG-X showed that the presence of the xanthate chain end on PEG was relevant, but also that the solids content that can be reached for a given polymerization time of the polymerization was linked to the number of hydrogenated species (in other words, the amount of PEG-X initially introduced). To emphasize the positive contribution of the reactive xanthate moiety on the formation of PVDF latex, experiments were designed with a lower molar mass PEG-X (Mn = 1300 g mol−1) or by introducing xanthate moieties on both chain ends (X-PEG-X, Mn = 3420 g mol−1) (Scheme 1). Experiment L07 in Table 1 was thus conducted with PEG-X of 1300 g mol−1 and the same KPS/PEG-X weight ratio as in L03. The number of xanthates moieties is thus doubled compared to L03 with a number of potential sites along the PEG chains for transfer reaction remaining the same (Scheme 3, case 1). The particle size obtained is smaller in L07 (62 nm) compared to L03 (72 nm) while the solids content remained unchanged (10.4%), leading to the formation of more particles (47.5 × 1016vs. 30.3 × 1016). As anticipated, this result shows the beneficial effect of favoring reversible chain transfer reaction on the xanthate chain ends over chain transfer along PEG backbone. In the same vein, decreasing the initial amount of PEG-X for a similar number of xanthate chain ends with respect to L03 (L08, KPS/PEG-X = 6.7, Scheme 3, case 2) effectively decreased the occurrence of irreversible chain transfer reactions leading to a 99 nm PVDF latex with a higher solids content (15.9%), in good agreement of the results obtained in experiment L06.
Scheme 3 Experiments performed with various amounts of PEG-X with different Mn (1300 or 2300 g mol−1). |
The positive impact of the reactive xanthate group on the particle stabilization was also demonstrated in a last experiment performed with X-PEG-X, keeping the KPS/X-PEG-X ratio to 2.5 (L09). This means that the number of xanthate moieties involved in this polymerization is twice the number involved in L03, for the same number of potential irreversible chain transfer sites along the PEG backbone (Scheme 3, case 3). This also means that if both xanthate moieties are efficiently reacting, the PEG chains will form loops on the particle surface. The particle size is similar for the two latexes (72 nm). However, the SC is lower in the case of L09 (8.5%) compared to L03 (10.5%). Larger particle size is thus expected for L09 for similar solids contents. The result is not against the formation of the expected two outer PVDF blocks at both PEG chain ends. However, the anchorage of the resulting amphiphilic structure onto the forming PVDF particles may disfavor the deployment of the hydrophilic part (PEG backbone with side PVDF grafts) of the corresponding stabilizer at the surface. The lower number of particles obtained for L09 (24.1 × 1016) compared to L03 (30.3 × 1016) might reflect a slightly lower stabilization efficiency.
The thermal properties of the PVDF polymers obtained using the different above-mentioned PEG-based species as stabilizer were investigated using DSC (Table S1†). The analyses showed that semi-crystalline polymers were formed, with Tm, Tc and Xc values in the range of what is commonly observed for PVDF polymers formed by emulsion polymerization.2,82
Eventually, experiment L01 and L03 in Table 1, performed with PEG-OH and PEG-X respectively, were scaled up in a 4 L reactor in experiments L10 and L11, respectively (Table 1). The solids content obtained after 4 h15 (7.6 wt% and 6.8 wt%) are similar to those for L01 and L03 (11.2 wt% and 10.4 wt%) although slightly lower. This probably accounts for the very different stirring and volume over surface ratios in the two sets of conditions. Nevertheless, it shows this technology is robust and that its transposition to a larger scale is possible.83
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1py00728a |
This journal is © The Royal Society of Chemistry 2021 |