Rana
Adel‡
a,
Elena
Gala‡
bc,
Matías J.
Alonso-Navarro
bc,
Edgar
Gutierrez-Fernandez
d,
Jaime
Martín
def,
Marco
Stella
g,
Eugenia
Martinez-Ferrero
g,
Alejandro
de la Peña
bc,
Alexandra
Harbuzaru
h,
M. Mar
Ramos
c,
Rocío Ponce
Ortiz
h,
José L.
Segura
*b and
Mariano
Campoy-Quiles
*a
aInstitut de Ciència de Materials de Barcelona, ICMAB-CSIC, Campus UAB, 08193, Bellaterra, Spain. E-mail: m.campoy@csic.es; mcampoy@icmab.es
bDepartamento Química Orgánica I, Facultad Ciencias Químicas, Universidad Complutense de Madrid, E-28040, Madrid, Spain. E-mail: segura@ucm.es
cDepartamento de Tecnología Química y Ambiental, Univ. Rey Juan Carlos, Móstoles, 28933, Spain
dPOLYMAT, University of the Basque Country UPV/EHU Av. de Tolosa 72, 20018, San Sebastián, Spain
eIkerbasque Basque Foundation for Science, Bilbao 48013, Spain
fUniversidade da Coruña, Grupo de Polímeros, Centro de Investigacións Tecnolóxicas (CIT), Esteiro, 15471 Ferrol, Spain
gEurecat Centre Tecnológic de Catalunya, Unit of Printed Electronics & Embedded Devices, 08302, Mataró, Spain
hDepartmento de Química Física, Universidad de Málaga, Málaga, 29071, Spain
First published on 7th January 2022
While it is widely recognized that microstructure plays an important role in the performance of organic photovoltaics (OPV), systematic studies are often challenging, as varying the molecular packing through typical chemical means (such as sidechain tuning) often affects the molecular energy levels, thus preventing a clear correlation. In this work we present the synthesis of three perylene imide (PI) based electron acceptors with almost identical energy levels, but distinct packing tendencies. We confirm our initial hypothesis by measuring solution and solid-state absorption, and cyclic voltammetry as well as characterizing the films by grazing incidence wide angle X-ray scattering (GIWAXS). In a second step, we repeat the characterization of the three materials in blends with two polymer donors, namely PCDTBT or PBDBT, whose energy levels are well aligned with those of the PI acceptors, and which, additionally, exhibit different degrees of structural order. We show how the initial strong difference between acceptors is partially blurred in blends, but still critical. Finally, we correlate our structural data with OPV devices made with the corresponding six blends. Our data suggest that a good donor acceptor marriage should ensure good energy alignment but also exhibit complementary crystallization tendencies of the two components.
Rylene imides such as perylene imides (PI)6 and naphthalene imide5–9 are among the most studied n-type materials in organic (opto)electronics because of their inherent electron deficient character which provides unique opportunities to conjugate electron-withdrawing moieties at different regions of a variety of π-scaffolds. Certainly, PIs are gaining great interest as non-fullerene acceptors in OPV devices and the photoconversion efficiencies (PCEs) of PI-based OPV systems have reached 9–10%.2,10–18 PIs are interesting materials not only because they absorb light in the visible region improving the light harvesting,19 but also because of their high photostability, low cost synthesis20 and adaptability to solution-processing. However, PI molecules have a high tendency to aggregate due to the π–π interactions between perylene cores, often leading to highly ordered column-like structures. The aggregation of the PI molecules has also an impact on their (opto)electronic properties.21 Thus, the formation of aggregates is considered as a source of charge carrier trapping,22 while changing morphology may affect the electrical conductivity in solid state films.23
The control of the morphology in OPVs based on PI molecules has been addressed by means of three different strategies:22 (i) by using block copolymers with inherent nanophase separation such as those reported by Laju Bu and co-workers with PCE of up to 1.5% that are based on monodisperse co-oligomers of electron donors with PIs;24 (ii) by precisely tuning the molecular architecture of perylene diimides (PDIs) as demonstrated by Rajaram and co-workers that obtained PCE values of 2.77% through combination of a hole-transporting polymer and a nonplanar PI derivative;25 (iii) by educated guesses aimed at controlling the crystallization in thin films of PI-based materials through variations in the processing conditions and partner polymers to achieve good compatibility between components. Unfortunately, rational guidelines to control the crystallization of PI derivatives in OPV blend films have not been established yet.
In this article, we report on the synthesis of a family of perylene imide-based electron acceptors with almost identical energy levels, but distinct molecular geometries and packing tendencies. The structure of the molecules can be finely tuned by using a common synthetic route starting from a functionalized perylene-imide derivative by reactions with different cores to yield PIPB which is planar molecule with monoatomic thickness, 3PIPT with a planar structure with monomolecular thickness based on the triptycene moiety, and 4PIPM with a three-dimensional structure based on the tetraphenylmethane core (Fig. 1). A combined study of their solid-state absorption and emission, together with the characterization of their electrochemical properties and the characterization of films by grazing incident wide angle X-rays (GIWAXs) is presented. In addition, blends based on the novel acceptors together with two polymer donors were also investigated. The two polymers, namely poly[N-9′-heptadecanyl-2,7-carbazole-alt-5,5-(4′,7′-di-2-thienyl-2′,1′,3′-benzothiadiazole)] (PCDTBT) and poly[(2,6-(4,8-bis(5-(2-ethylhexyl)thiophen-2-yl)-benzo[1,2-b:4,5-b′]dithiophene))-alt-(5,5-(1′,3′-di-2-thienyl-5′,7′-bis(2-ethylhexyl)benzo[1′,2′-c:4′,5′-c′]dithiophene-4,8-dione))] (PBDBT) (Fig. 1), have energy levels well aligned with those of the PI acceptors, and, additionally, exhibit different degree of structural order.26 The characterization of the three electron acceptor materials in blends with the two polymer donors allows us to analyse the impact of the different initial molecular stacking tendency on the resulting blend microstructure, and how the latter affects photovoltaic performance. While final device efficiencies are modest, we can still establish interesting connections between single component microstructure and that of the corresponding blend, as well as ideas on how to choose blend partner in terms of microstructure compatibility.
Fig. 1 (a) Synthesis of PIPB, 3PIPT and 4PIPM; the molecular structure of (b) PCDTBT, (c) PBDBT and (d) the energy levels of all the molecules deduced from cyclic voltammetry and UV-Visible. |
The optimization of the lowest energy molecular structures of the novel NFAs was accomplished by using the DFT exchange correlation functional B3LYP/6-31* level. Long branched alkyl chains at the imide groups are replaced by methyl groups to simplify the calculations. For the linear compound PIPB, the frontier molecular HOMO and LUMO orbitals are spread all over the molecule, as it has already been observed for other similar compounds.28 In the case of 3PIPT, the HOMO is spread over the three perylene cores whereas, the LUMO/LUMO+1 orbitals are found to be degenerated due to molecular symmetry. As a consequence, the combination of the two degenerated orbitals also shows wave function delocalization over the three branches.29,30 Note, however, that minimal contribution of the triptycene central unit to the frontier molecular orbitals is observed (Fig. 2). The absence of the triptycene contribution to the frontier molecular orbitals precludes the homoconjugation effect already observed in other iptycene derivatives.31,32 For 4PIPM, a similar scenario is found, where the tetraphenylmethane core minimally contributes to the frontier molecular orbitals.
Fig. 2 (a) G16 DFT/B3LYP/6-31* optimized molecular structures for the semiconductors under study and (b) molecular orbital topologies of PIPB (left), 3PIPT (middle) and 4PIPM (right). |
To gain some insight into the electrochemical and optical properties of the three NFAs, they were characterized by cyclic voltammetry and UV-Visible and fluorescence spectroscopies. Table 1 summarizes all the relevant data, including the experimental LUMO and HOMO energies obtained from the electrochemical and optical studies.
Acceptor | λ abs | ε | λ onset | E g | λ em | E 1/2redIe | E 1/2redII | E LUMO | E HOMO |
---|---|---|---|---|---|---|---|---|---|
a Wavelength in nm in CHCl3 solution. Maxima italicized. b Shoulder. c Molar extinction coefficient in M−1 cm−1 at λmax in solution. d Energy band gap (in eV) derived from the low-energy absorption edge. e Values in V estimated from cyclic voltammetry in DCM/TBAPF6 (0.1 M) at a scan rate of 0.15 V s−1 using Pt as working and the counter electrode and Fc/Fc+ as reference. f Values in eV, estimated from ELUMO = −5.1 eV − E1/2redI. g Values in eV, estimated from EHOMO = ELUMO − Eoptg. | |||||||||
PIPB | 323, 364, 379, 463, 496, 534 | 1.67 × 105 | 555 | 2.23 | 545, 588, 637b | −1.26 | −1.44 | −3.84 | −6.07 |
3PIPT | 337, 395, 470, 501, 540 | 3.26 × 105 | 566 | 2.19 | 548, 592, 640b | −1.16 | −1.38 | −3.94 | −6.13 |
4PIPM | 331, 368b, 388, 471b, 503, 541 | 3.14 × 105 | 587 | 2.11 | 546, 590, 638b | −1.14 | −1.39 | −3.96 | −6.07 |
Redox potentials were determined as the midpoints of the forward and reverse scans in cyclic voltammograms (Fig. 3b) carried out in dichloromethane solutions in a standard electrochemical cell where platinum electrode, platinum–wire electrode and Ag/Ag+ electrode were used as working electrode, auxiliary electrode and reference electrode, respectively. Tetrabutylammonium hexafluorophosphate (0.1 M) was used as the electrolyte and potentials were recorded versus Fc/Fc+. The fingerprint of the cyclic voltammetry characterization of peryleneimides involves the presence two sequential one-electron cathodic waves, corresponding to the formation of the radical anion and the dianion, respectively.33 For systems bearing more than one ryleneimide moiety, the number of redox processes observed is related to the electronic communication or lack of electronic communication between the rylenemimide moieties. Thus, the splitting of the reduction potentials is indicative of electronic communication between ryleneimide redox centers.34 In contrast, only two distinct reversible waves are observed in assemblies with several ryleneimide moieties without electronic communication between the ryleneimide redox centers.35 For PIPB, 3PIPT and 4PIPM, only two sequential reduction processes (Fig. 3b) are observed in their cyclic voltammetry measurements thus indicating that the peryleneimide moieties reduce simultaneously to the corresponding radical anions and dianions due to the lack of significant electronic communication between the peryleneimide moieties in the multichromophoric systems (3PIPT and 4PIPM). The potential values obtained for these processes lie in the range of those observed for good n-type semiconducting materials.36
From the first reduction potentials obtained by the cyclic voltammetry measurements it is possible to estimate the LUMO energies of the novel arylenimide assemblies by using standard approximations.37,38 Because no oxidation processes could be detected within the solvent/electrolyte window (Fig. S25, ESI†), it is not possible to estimate the HOMO energies from the oxidation potentials. However, they can be estimated by using the LUMO energies and the optical band gaps by using the equation EHOMO = Eoptg + ELUMO.39 Accordingly, for these three new systems, the estimation of the lowest unoccupied molecular orbital (LUMO) energies are −3.84 eV, −3.94 eV and −3.96 eV for PIPB, 3PIPT and 4PIPM and the values estimated for the highest occupied molecular orbital (HOMO) energies are −6.07 eV, −6.13 eV and −6.07 eV for PIPB, 3PIPT and 4PIPM (Table 1).
UV-Vis and fluorescence spectra were recorded in chloroform solutions and the data obtained are summarized in Table 1. Characteristic absorption bands of perylenimide derivatives were observed for the three novel NFAs. For PIPB, the peaks with the highest intensities can be observed at 497 nm and 535 nm corresponding to the 0–0 and 0–1 vibronic bands of the S0–S1 transition. On the other hand, the band with a maximum at 465 nm can be ascribed to the electronic S0–S2 transition (Fig. 3a). A similar pattern but slightly red shifted can be observed in the UV-vis spectra of systems with higher dimensionality 3PIPT and 4PIPM. The concentration-dependent UV-vis absorption spectra of these compounds in chloroform shows a bathochromic shift and the (0,1) vibronic band shows an increase relative to the (0,0) transition (Fig. S21–S23, ESI†). This is a typical behaviour of aggregated perylenimide chromophores. Strong vibronic coupling in the aggregates results in an enhanced (0,1) vibronic band compared to non-aggregated PDI molecules. Thus, upon aggregation of PDI derivatives, the ratio of the intensities of the (0,0) and the (0,1) transitions decreases, which is often used as an indication of aggregation40–44 that can be rationalized by the molecular exciton model.45–47 This behaviour is especially remarkable for 4PIPM for which the effect of self-aggregation could be observed even at concentrations as low as 10−7 M. The molar extinction coefficient (ε) estimated for PIPB was 167197 M−1 cm−1, almost half of that observed for the derivatives with higher dimensionality: 326029 M−1 cm−1 for 3PIPT and 313757 M−1 cm−1 for 4PIPM (Table 1). Emission spectra were also recorded in chloroform solutions and the bands observed correspond to the emission from the lowest energy transitions described for the absorption spectra (Fig. S24, ESI†).
The optical properties of the novel semiconductors were also investigated in the solid state by UV-vis and fluorescence spectroscopies. Thin films of PIPB, 3PIPT and 4PIPM were prepared by blade coating from chloroform:chlorobenzene (CF:CB 3:1 VR) solutions. (This mixture of solvents was found to lead to the highest efficiencies in OPVs based on these materials, as we will explain below). Solid-state UV-Vis spectra confirmed the high tendency of the new acceptors to form aggregates. For PIPB, a bathochromic shift of 55 nm and an inversion of the relative intensities of the absorption signals corresponding to the (0,0) and (0,1) transitions were observed in comparison with that observed in the solution spectrum (Fig. 3c). On the other hand, for the three-dimensional derivatives, 3PIPT and 4PIPM, the only noticeable change observed was the inversion of the relative intensity of the aforementioned bands (Fig. 3c). The thin film photoluminescence spectra of PIPB, 3PIPT and 4PIPM are shown in Fig. 3d. After laser excitation at 633 nm, the three systems show emission up to 900 nm, with emission maxima at 721 nm for the three systems. An additional relative maximum peaking at 673 nm was observed only for PIPB.
The solid-state molecular packing of PIPB, 3PIPT and 4PIPM was studied by grazing-incidence wide-angle X-ray scattering (GIWAXS). Shown in Fig. 4 are the 2D patterns obtained and their corresponding intensity profiles along the out-of-plane (OOP, z) and in plane (IP, r) directions. The pattern for the mono-adduct PIPB shows distinctive oriented and well-defined Bragg peaks, denoting a significant degree of crystallinity. Because the peak showing up at qr = 18 nm−1 (d ∼ 0.35 nm) along the in-plane direction is presumably associated with the π–π stacked planes, we argue that molecules in this sample are oriented edge-on with respect to the substrate. For the higher dimensionality adducts, i.e.3PIPT and 4PIPM, the formation of well-ordered structures seems to be hindered. Thus, the GIWAXS pattern for 3PIPT exhibits broad, isotropic reflections, characteristic of an eminently disordered packing. Interestingly, the compound with four perylenimide units, 4PIPM, features some degree of regular packing, as suggested by the presence of a weak peak at qz = 3.5 nm−1 and a noticeable bump at qz = qr = 17.5 nm−1. Hence, our analysis reveals a different degree of lamellar packing in the neat films of the 3 compounds, ranging from an amorphous and isotropic structure for 3PIPT to highly crystalline films for PIPB films. The above packing behaviour can be rationalized by considering that the planar structure of PIPB allows for the formation of well-ordered films through π–π stacking. On the other hand, 4PIPM has four branches linked to the tetraphenylmethane core by single bonds, and thus are relatively free for rotations around several planes, which we propose that helps the molecule to induce a certain lamellar packing and a weak π–π stacking. Finally, in 3PIPT the three branches are fixed perpendicular to the main plane of the molecule, which hinders molecular motion during solidification, thus leading to an overall amorphous structure.
1:1 (weight ratio) polymer:NFA films were prepared from CF:CB (3:1 VR) solutions. The UV-Vis absorption spectra of these films were normalized to the film thickness and showed absorption bands in the same range as those observed for the pure donor polymer and the NFAs (Fig. 5a and 6a). For PCDTBT, two absorption bands can be observed (Fig. 5a). A high energy band that is ascribed to the N-(1-octylnonyl)-2,7-di(thien-2-yl) carbazole unit and a low-energy band (LEB) which has intramolecular charge transfer (CT) character. As the three NFAs also exhibit two absorption bands in approximately the same spectral regions, the absorption of the blends is relatively similar to that of the polymer alone. For mixtures containing PIPB and 3PIPT, a small red shift can be, however, detected. Moreover, the thickness normalized absorption data suggest that PCDTBT:3PIPT blends exhibit a stronger absorption compared to the other systems.
Photoluminescence spectra of blend films containing the PCDTBT were registered under illumination with a 633 nm laser source. PL intensity was normalized to the corresponding optical absorption at the excitation wavelength (Fig. 5b). The interaction between the NFAs and the PCDTBT polymer resulted in a shift of the emission band, which peaked at 715 nm for the pristine NFAs films (Fig. 3), and peaked at 720, 713 and 759 nm for PCDTBT:4PIPM, PCDTBT:3PIPT and PCDTBT:PIPB, respectively (Fig. 5b). On the other hand, a PL emission maxima of 697 nm was observed for the pristine PCDTBT polymer film. Interestingly, the extend of red shift correlates with the crystallization tendency of the three systems. Indeed, the above results can be rationalized in terms of (i) small-molecule intermolecular aggregation and (ii) polymer-small-molecule interactions. The most significant bathochromic shift observed for the PCDTBT:PIPB films could be understood as the result of an efficient aggregation of the planar acceptor molecules by π–π stacking, promoted by the dilution effect granted by the polymer matrix. For PCDTBT:3PIPT films, even an effective slight hypsochromic effect is observed, which can be related to a better acceptor–donor interconnection likely due to the reduced tendency of 3PIPT towards aggregation (Fig. 4). The effect is, however, very small, and it could be also explained by the overlap of the donor and acceptor PL spectra. The slight red shift observed in the spectrum of the PCDTBT:4PIPM film reveals an intermediate degree of PL shifting, also correlating with a less significant aggregation tendency of this three-dimensional acceptor molecules by π–π stacking compared to PIPB. At this stage, we cannot fully rule out another potential explanation for the observed trend, which would be reabsorption by the crystalline domains, preferentially absorbing the lowest energy photons emitted.
The GIWAXS shows that the three donor:acceptor pairs, i.e.PCDTBT:4PIPM, PCDTBT:3PIPT and PCDTBT:PIPB, exhibit low degrees of structural order. We conclude the above from both the 2D patterns in Fig. 5c–f and the corresponding OOP and IP line cuts in Fig. 5g–j, which, in general, display broad and isotropic diffraction maxima. Neat PCDTBT, 4PIPM and 3PIPT have little tendency to arrange into structurally ordered structures as demonstrated above, hence, it is reasonable that they retain this behaviour also in blends. More striking is, however, the strong vitrification of the PIPB compound after blending with PBDBT, which is likely due to thermodynamic reasons.49 Nevertheless, a detailed inspection of the pattern of the PBDBT:PIPB blend reveals weak peaks at qz = ∼9 nm−1 and qr = 17.5 nm−1 that likely originate from the presence of fractions of some structurally ordered NFAs in this blend.
The polymer PBDBT, which exhibits a higher degree of structural order than PCDTBT, was also used to prepare blend films with the three novel NFAs acceptors. These blends were also prepared from 1:1 polymer:NFA solutions in CF:CB (3:1 VR) solutions. As before, optical properties of the films were studied by UV-Vis and PL spectroscopy (Fig. 6a and b). In contrast to the PCDTBT:NFA blend films, no major differences can be observed in the different NFAs.
Photoluminescence spectra of blends containing PBDBT resulted in a general red shift and broadening of the emission band centred at 715 nm for the NFAs films (Fig. 3) and that at 736 nm for the pristine PBDBT polymer film (Fig. 6). Thus, emission bands were observed at 767, 772 and 773 nm for PBDBT:4PIPM, PBDBT:3PIPT and PBDBT:PIPB, respectively (Fig. 6). The PL spectra of PBDBT is clearly of low intensity indicating the high order presents in the polymer as a result of the aggregation caused quenching (ACQ) phenomena. In ACQ, non-radiative relaxation resulted in planar molecule that arises from the short π–π stacking.50–52 The observed red shift and broadening of the bands suggest the formation of aggregated structures. The higher degree of structural order of PBDBT in comparison with PCDTBT can favour the formation of phase separation due to the formation of microstructure islands in PBDBT-based films which may be responsible for the reduced photoluminescence intensity observed for PBDBT-based films in comparison with the PCDTBT analogues. Alternatively, the absorption of the polymer itself, which goes well down 700 nm, could introduce some degree of self-absorption in all films. Strong emission from a charge transfer at the donor/acceptor interface is, however, unlikely due to the degree of phase separation (vide infra).
In good agreement with PL data, GIWAXS patterns for all the blends show essentially the reflections observed in neat PBDBT films (Fig. 6c–h), which suggests, again, that NFAs arrange in disordered domains also in these blends. However, similarly to the PCDBTB:PIPB blends discussed, a close view of the pattern for PBDBT:PIPB reveals some weak signals at qr = 3.5 nm−1 and qr = 17.5 nm−1 along the in-plane direction that can originate from crystalline NFA domains. The presence of distinctive diffraction peaks and PL peaks associated with both the NFA and the polymer indicates the existence of a phase separated nanomorphology in the PBDBT:PIPB blend. This blend seems to include, likely among other phases, structurally ordered polymeric domains and crystalline NFA domains. For PBDBT:4PIPM and PBDBT:3PIPT binary blends, phase separated domains can be also presumed according to PL data, but NFA domains seem to be amorphous in these cases, according to GIWAXS results.
Raman spectroscopy was used to further investigate the microstructure and to address any chemical change that might be produced during the processing of the PCDTBT:NFA blend films. Comparison between the Raman spectra of the small acceptor molecules, PCDTBT and PCDTBT:NFA blend films strongly suggests that the structure of the NFAs and PCDTBT remain unaltered after the film processing (see Fig. 7 and Table S1, ESI†). However, the shifts and splitting of peaks observed in the blend films (Table S1, ESI†) indicate a strong interaction between the polymer and the small molecules in agreement with that previously observed in the photoluminescence study. While a full theoretical assignments of peaks has not been carried out, we would like to point out a few observations. For blends including PCDTBT as the polymer, the polymer peaks related to the backbone (between 1300 and 1700 cm−1) tend to shift to higher wavenumbers. For instance, the 1348 cm−1 and 1541 cm−1 peaks of the polymer go to 1352 cm−1 and 1543 cm−1, respectively, when mixed with 3PIPT. This vibration hardening is typically resulting from the polymer reducing its degree of order and is typical of conjugated polymers upon blending.53,54 In the case of PBDBT, it is interesting to notice that many of the peaks cannot be properly resolved upon blending. On the other hand, the peaks of the NFAs that can be independently resolved from those of the polymers seem to be less affected by blending with PCPTBT than with PBDBT. Blending with PBDBT has, indeed, a stronger effect on the peaks associated to the NFAs, shifting them, in most cases, to lowers wavenumbers. This would suggest that, at a single molecule level, the dielectric environment of the molecules is very much affected by the degree of order of the polymer matrix, having a greater effect with increased order.
Fig. 8 (a) The J–V curves of the champion PV devices with PCDTBT donor polymer and (b) the J–V curves of the champion PV devices with PBDBT donor polymer. |
Heterojunctions | V oc (V) | J sc (mA cm−2) | FF (%) | PCE (%) |
---|---|---|---|---|
PCDTBT:4PIPM | 0.88 ± 0.06 (0.92) | 1.46 ± 0.03 (1.44) | 32 ± 2 (33) | 0.41 ± 0.04 (0.44) |
PCDTBT:3PIPT | 0.7 ± 0.2 (0.8) | 2.2 ± 0.1 (2.3) | 33 ± 3 (30) | 0.49 ± 0.11 (0.56) |
PCDTBT:PIPB | 1.16 ± 0.01 (1.16) | 3.02 ± 0.01 (3.02) | 32 ± 4 (35) | 1.12 ± 0.14 (1.22) |
PBDBT:4PIPM | 0.75 ± 0.01 (0.75) | 2.3 ± 0.1 (2.4) | 41 ± 1 (41) | 0.73 ± 0.01 (0.74) |
PBDBT:3PIPT | 0.79 ± 0.04 (0.82) | 2.45 ± 0.08 (2.5) | 40 ± 4 (42) | 0.76 ± 0.13 (0.85) |
PBDBT:PIPB | 0.88 ± 0.01 (0.87) | 2.0 ± 0.2 (2.2) | 25 ± 1 (26) | 0.43 ± 0.07 (0.48) |
First, the devices were fabricated blending the small molecules with the less crystalline polymer donor, PCDTBT. The device performance varied depending on the nature of the acceptor used (Fig. 8 and Table 2). The best PCE value obtained was 1.22% for the device based on the PCDTBT:PIPB blend. Lower performances were obtained for devices fabricated with PCDTBT:4PIPM (0.44%) and PCDTBT:3PIPT (0.56%) blends after a thickness, ratio and annealing optimization process. We have used the high throughput method for screening the thickness following the previous work (see Tables S2 and S3, ESI†).55 For the three devices the overall values of the fill factors (FF) were in the 29–33% range. These very low values can be the result of the low packing order in the blend films that prevents a good charge transport. Furthermore, considering the energy level of the three acceptor molecules and the low fill factor of the devices, the analysis of the open circuit voltages (Voc) values (Fig. S27, ESI†) indicates the existence of microstructure-related recombination. This observation is consistent with previously reported studies that show an increase in the charge carrier mobility when crystalline electron donors are mixed with less crystalline acceptors thus enhancing the FF and photoconversion efficiency (PCE) in the device.56 In blends containing electron donor polymers and PDI derivatives as electron acceptor units the trap assisted charge recombination loss is likely enhanced,21 and in the blends with PCDTBT electron donor polymer the formation of trapping sites cannot be avoided independently of the three-dimensional orientation of the PDI acceptor units. In the particular case of PCDTBT:PIPB, an enhancement on the electron transport can be expected as a consequence of the intermolecular π–π stacking of the PIPB moieties in the polymeric matrix.
Blend films containing the PDI-based electron acceptors and the more structurally ordered polymer, PBDBT, as donor, have also been evaluated as active layers in OPV devices. The efficiency of the devices built with the PBDBT:PIPB blend film were lower in comparison with that measured for the analogous device built with a PCDTBT:PIPB film (0.48% vs. 1.2%). Slightly higher efficiencies were found for the devices fabricated with the PBDBT:4PIPM (0.74%) and PBDBT:3PIPT (0.85%) heterojunctions (see Table 2). The average fill factors determined for devices built with PBDBT:4PIPM (41%) and PBDBT:3PIPT (42%) blend films were higher than those obtained with the partner blends based on the less crystalline PCDTBT polymer (PCDTBT:4PIPM (33%) and PCDTBT:3PIPT (30%)). In contrast, the FF values of devices built with PBDBT:PIPB (26%) were similar to those obtained for devices fabricated with PCDTBT:PIPB blend films (35%) (Table 2). Eventually the 4PIPM and 3PIPT behave similarly in the devices unlike the PIPB that shows a clear change in the device performance when combined with the two polymer donors. The device parameter trends obtained correlate relatively well with the structural information extracted from the combined study of the UV-vis absorption, fluorescence and GIWAXS data outlined above and highlight the importance of the microstructure of the heterojunctions. More specifically, our data shows that PIPB has a stronger tendency to pack into ordered structures when blended with PBDBT, which likely results in a more phase separated morphology that encompasses isolated, non-percolated microislands that penalize charge transport and, hence, the device efficiency.57
The results summarized above have focused on films and OSC devices prepared from solutions of the components in CF:CB 3:1 VR mixtures. In order to investigate the origin of the relatively low efficiencies, we studied the effect of the solvent on the performance of the systems under consideration. By using chloroform, chlorobenzene and their mixtures in different proportions, we observed that the solubility of the small molecules is a crucial parameter to be considered (Fig. S27 and S28, ESI†). Despite the lower solubility of the NFAs in chloroform (CF), the use of CF as co-solvent together with dichlorobenzene (CB) improves the performance of the devices in comparison with the use of pure CB. This behaviour can be ascribed to the drying time since the low boiling temperature of CF leads to faster drying and partially prevents large scale phase separation in comparison with processing only with CB. Further investigation of the solvent influence on performances of the devices based on the six different heterojunctions (PCDTBT:4PIPM, PCDTBT:3PIPT, PCDTBT:PIPB, PBDBT:4PIPM, PBDBT:3PIPT and PBDBT:PIPB) was also accomplished in connection with the Hansen solubility parameters (polarity, hydrogen bond and dispersion) by ANOVA statistical analysis (Table S4, ESI†).52,58–63 We find that the polarity has F factor of 71.4, hydrogen bonds and the dispersion coefficients have the same value of 114.8. Since the Hansen parameters shows high dispersion of the efficiency of the devices, the surface map of photovoltaic device efficiencies to Hansen solubility parameters for different solvents used for the active layer formation TCE: tetrachloroethane, DCM: dichloromethane, CB: chlorobenzene and CF: chloroform is shown in Fig. S29 (ESI†). These findings indicate that a polar solvent like chloroform improves the solubility of the active layer components and results in better performance than CB. DCM and TCE result in less efficient device performance than the combination between chloroform and chlorobenzene (3:1) VR.
These findings increase the awareness of future investigations toward the benefits of optimizing the π–π intermolecular stacking for enhancing the efficiency of the charge separation and hence improving the photogenerated current in heterojunctions. This can be addressed by increasing the density of grain boundaries of the small PDI crystallites while the generated electrons travels through the interconnected small PDI aggregates to reach the electrode.64
Raman and PL spectra of the blend films, prepared by blade coating on glass substrate, were measured using a Witec alpha300RA. For Raman, the scanned area was 0.25 mm2 with scanning resolution of 10 points per line, 10 line per image, scan speed 2 s/line and integration time of 0.23 s. As excitation, we used a 488 nm solid state laser source with a power of 1 mW for Raman, and a 633 nm HeNe laser for PL. The gratings were 1200 g m−1 and 300 g m−1 for Raman and PL, respectively.
Dedicated to the memory of our friend and colleague Prof. Alasdair Campbell.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1tc05037k |
‡ These authors contributed equally to this work. |