Open Access Article
Hyuntae
Bae
a and
Youngsik
Kim
*ab
aSchool of Energy and Chemical Engineering, Ulsan National Institute of Science and Technology (UNIST), Unist-gil 50, Ulsan, 44919, Republic of Korea
bEnergy Materials and Devices Lab, 4TOONE Corporation, UNIST-gil 50, Ulsan, 44919, Republic of Korea
First published on 28th April 2021
The consumption of lithium-based materials has more than doubled in eight years due to the recent surge in demand for lithium applications as lithium ion batteries. The lithium-ion battery market has grown steadily every year and currently reaches a market size of $40 billion. Lithium, which is the core material for the lithium-ion battery industry, is now being extracted from natural minerals and brines, but the processes are complex and consume a large amount of energy. In addition, lithium consumption has increased by 18% from 2018 to 2019, and it can be predicted that the depletion of lithium is imminent with limited lithium reserves. This has led to the development of technologies to recycle lithium from lithium-ion batteries. This article focuses on the technologies that can recycle lithium compounds from waste lithium-ion batteries according to their individual stages and methods. The stages are divided into the pre-treatment stage and lithium extraction stage, while the latter is divided into three main methods: pyrometallurgy, hydrometallurgy, and electrochemical extraction. Processes, advantages, disadvantages, lithium extraction efficiency, price, environmental pollution and the degree of commercialization of each method are compared and analyzed quantitatively. Despite the growing attention and the development of various lithium recycling technologies, less than 1 percent of lithium is recycled currently. We propose future needs to improve the recycling technologies from waste lithium materials and hope that this article can stimulate further interest and development in lithium recycling.
For these reasons, lithium is expected to become more valuable, highlighting the importance of lithium recycling. This paper explains the current state of lithium and emphasizes the importance of lithium recycling. In addition, this paper lists the various techniques used for lithium recycling, along with the process, advantages, and drawbacks of each method and concludes with recommendations for research and development in lithium recycling technologies.
![]() | ||
| Fig. 1 (a) Distribution of total lithium usage in 2019; (b) distribution of global lithium resources. | ||
Lithium is preferred as the material for batteries owing to three properties: (1) it is the lightest metal (2) it has the highest electrochemical potential of all metals, and (3) it has the highest energy density among all metals.13 In addition to batteries, lithium is also used in ceramics, glass, and greases/castings with particular chemical properties. Adding lithium to ceramics increases the glass melt rate and decreases their viscosity and melt temperature. Additionally, the high thermal expansion coefficient of lithium makes ceramics resilient to heat shock and increases mechanical strength.14 Lithium grease is useful in concentrating oil to produce high-temperature grease,15 and lithium additives are used in casting to increase fluidity.16 Organic lithium materials are used as strong bases in polymers to form carbon–carbon bonds.17
Lithium is extracted from two natural sources: ores and salt lakes. Lithium can be extracted from spodumene, petalite, and eucryptite, and the composition of the lithium in these ores ranges from 2% to 5.5%20 (Table 1). The minerals are crushed, separated by gravity flotation, concentrated, and heat-processed for water leaching, acid treatment, and pressure leaching to produce the lithium solution. Na2CO3 was added to the lithium solution to extract lithium sediments.18,21,22
| Ore | Chemical formula | Li contained (wt%) |
|---|---|---|
| Spodumene | LiAlSi2O6 | 3.73 |
| Petalite | LiAlSi4O10 | 2.09 |
| Amblygonite | (Li,Na)AlPO4(F,OH) | 3.44 |
| Lepidolite | K(Li,Al)3(Si,Al)4O10(F,OH)2 | 3.58 |
| Eucryptite | LiAlSiO4 | 5.51 |
The second method for extracting lithium is from a salt lake or brine. Lithium brines exist in Argentina, Bolivia, Chile, China, and the USA.21 The lithium grade and magnesium/lithium ratio of the brine are important factors that affect the production cost and time.23–28Table 2 lists the lithium content and Mg/Li ratio of the brines currently used in production.21 Brine contains 0.02 to 5% Li+, along with other ions such as Na+, K+, Cl−, and SO42−.27 Lithium is extracted from brine using the precipitation method. Water is evaporated from the brine in a solar pond, followed by the precipitation of NaCl and KCl, and the concentration of lithium in the solution. Next, Ca(OH)2 is added to the concentrated lithium brine to remove Mg and sulfate via precipitation. The remaining Ca and Na2CO3 in the concentrate are removed via precipitation using CaCO3. This fluid then undergoes filtration and washing and is heated to 80–90 °C to react with Na2CO3 and form Li2CO3.27 (Fig. 2) While solar evaporation followed by precipitation is a popular method, the procedure is time-consuming, lasting from 18 to 24 months.28 For brines with a high Mg/Li ratio, Al is used to precipitate lithium–aluminate. This method exhibits superior lithium separation and precipitation rates.29 This method involves the addition of AlCl3, H2O, NaOH, and amorphous Al(OH)3, followed by adjusting the temperature and pH to extract lithium as LiAlO2 (eqn (1)).
| LiCl + 2AlCl3 + 6NaOH → LiCl·2Al(OH)3 H2O + 6NaCl | (1) |
| Salt lake | Country | Li contained (%/ton) | Mg/Li |
|---|---|---|---|
| Atacama | Chile | 0.15 | 6.4 |
| Hombre muerto | Argentina | 0.062–5 | 1.37 |
| Rincon | Argentina | 0.033 | 8.61 |
| Uyuni | Bolivia | 0.035 | 18.6–21.5 |
| Silver peak | USA | 0.023 | 1.43 |
| Zhabuye lake | China | 0.12 | Low |
| DXC salt lake | China | 0.04 | 0.22 |
![]() | ||
| Fig. 2 Process example of Lithium extraction processes from natural lithium brine via chemical precipitation. | ||
While extracting lithium from ores ensures higher lithium concentration, the production cost is higher than that of brine extraction because of the more energy-intensive procedure. Thus, 87% of lithium is produced by brine extraction.30 Lithium also exists in seawater, which is quite abundant, but its concentration is too low (0.17 ppm) to be economical.31,32 However, there are ongoing research efforts to reduce the cost of lithium extraction.
000 dollar per metric tons in 201833 (Fig. S1, ESI†). There has been a steady increase in the adoption of lithium-battery-powered personal electronics, electronic vehicles (EVs), and ESS owing to the thrust on green energy. These trends have expanded the lithium-ion battery market to $44 billion in 2020.34 The growth in the ESS and EV battery markets has further accelerated this expansion. To illustrate the potential increase in demand, it must be noted that while smartphones, laptops, and tablets contain approximately 2 g, 6 g, and 20 g of lithium per device, respectively,35 an EV battery requires approximately 20 kg of lithium, which is 1000 times that of a smartphone, and a 10 MWh ESS requires at least 700 kg of lithium.35,36 As the demand for lithium-ion batteries increases, the increase in lithium prices can weaken the lithium-ion battery market.
Lithium consumption rose from 49
100 tons in 2018 to 57
700 tons in 2019, registering an increase of 18%.37 Global lithium reserves are estimated to be approximately 17 billion tons. If the 18% annual increase in consumption continues, global lithium reserves will be exhausted. In 30 years, the demand for lithium will be approximately 63 million tons, which will be 40 million tons more than the remaining reserves (Fig. 3). Although more lithium reserves may eventually be discovered, the increase in demand is predicted to accelerate owing to the expanding market for lithium-ion batteries. An increasing number of agencies across the world forecast shortages of lithium and these predictions have gained much research interest in recent years.38,39
![]() | ||
| Fig. 3 Global lithium reserves and lithium depletion scenario after 30 years when lithium consumption increasing rate is 18% per year. | ||
A lithium-ion battery can last up to three years in a small electronic device, and from five to ten years in a larger device; this is shorter than the lifespan of other batteries, considering that Ni–Cd batteries last from fifteen to twenty years, and lead-acid batteries last from five to ten years.40–44 Currently, 80% of lithium-ion batteries are used for small electronics, with EV and ESS applications accounting for less than 20%.45 Lithium-ion battery disposal was estimated to be 10
700 tons in 2012.46 This value has increased progressively each year, with an estimate of up to 250
000 tons in 2020.45 With the large-scale adoption of EVs and ESSs, the number of lithium-ion batteries in service is expected to increase. Discarded lithium-ion batteries are collected by government authorities or companies authorized by the manufacturer. Consumers normally dispose of lithium-ion batteries in a government-designated area or these are directly collected by the relevant agency. However, only 2–5% of lithium-ion batteries are collected in Australia, the EU, and the US47 (Fig. 4). The reason for the low collection rate is the lack of consumer awareness, as well as the tendency to resell electronics rather than recycle them. Although it may vary by country, there is a lack of legal and physical infrastructure for widespread collection and efficient, safe, and economical transportation of the disposed lithium-ion batteries. Major improvements are required to significantly increase the collection rate.
Recycling of lithium-ion batteries has been steadily researched since the 1990s and has recently gained traction. However, most research focuses not on lithium but on more expensive materials, such as cobalt. Therefore, little focus has been placed on extracting lithium from disposed batteries. Cobalt is the most expensive material in a lithium-ion battery; thus, there has been considerable research interest in reducing the cobalt content or replacing it by using LiFePO4 or LiNi0.3Mn0.3Co0.3O2.48 However, lithium is an irreplaceable key component in lithium-ion batteries, and it is used in the cathode, electrolyte and anode. Therefore a comprehensive review of the recycling of lithium from lithium-ion battery recycling is needed.
Lithium can be extracted from a lithium-ion battery via two major processes. Owing to the difficulty of separating lithium from the packed battery, the disposed battery is subjected to a pre-treatment process to separate the lithium-containing active material(cathode, anode) from the peripheral parts(plastic, polymer). Next, lithium is chemically separated from the active materials using pyrometallurgy, hydrometallurgy and electrochemical extraction methods (Fig. 5). The two processes, pre-treatment and lithium extraction, are explained.
![]() | ||
| Fig. 5 Schematic diagram of the overall lithium recycling stages and methods from discarded lithium-ion batteries. | ||
![]() | ||
| Fig. 6 Example of pre-treatment technology and processes of waste LIBs; (a) mechanical (b) solvent treat and (c) calcination. | ||
Various methods can be used to pre-treat discarded lithium-ion batteries. Each method has its advantages and drawbacks, and a more scalable method needs to be developed for use on a commercial scale. Table 3 lists the results and conditions of the different pre-treatment methods.
| Method | Residue | Condition | Ref. |
|---|---|---|---|
| Mechanical | Al, Cu/LCO/graphite | • Discharge, blade crusher 3000 rpm/20 s | 52 |
| Mechanical | Active materials | • Hammer mill (10 mm), spouted bed elutriation | 53 |
| Mechanical | Electrode powders | • Granulator machine/10 min | 54 |
| Mechanical | Cathode powders | • Granulator machine/10 min, shredding | 55 |
| Mechanical | Electrode powders | • Discharge, twin-shaft shredder | 56 |
| • Hammer mill (5 mm control grid)/10 min | |||
| • Granulator machine/10 min | |||
| Mechanical | Active materials | • Discharge, vertical impact crusher | 57 |
| • Sieving and screening | |||
| • Falcon series centrifugal concentrator | |||
| Solvent | Cathode powders | • Discharge, manually dismantling and separation | 58 |
| • NMP 60 °C/1 h, 700 °C/5 h | |||
| Solvent | Cathode powders | • Discharge, manually dismantling and separation | 59 |
| • Ultrasonication in NMP, 800 °C/2 h | |||
| Solvent | Cathode powders | • Manually dismantling and separation | 60 |
| • NMP, ultra-sonication 80 °C/2 h | |||
| Solvent | Cathode powders | • Manually dismantling and separation | 61 |
| • NMP, 100 °C/2 h, 700 °C/2 h | |||
| Thermal | Cathode powders | • Discharge, manually dismantling and separation | 62 |
| • Vacuum pyrolysis | |||
| Thermal | Active materials | • Discharge, manually dismantling and separation | 63 |
| • 300 °C/30 min | |||
| Thermal | Cathode powders | • Dismantling and separation | 64 |
| • 500 °C, ANVIL (air-jet-separation) | |||
| Thermal | Active materials | • Discharge, manually dismantling and separation | 65 |
| • 600 °C/15 min in N2 condition |
| C + 12LiMO2 → 6Li2O + 4M3O4 + CO2 | (2) |
| C + 4LiMO2 → 2Li2O + 4MO + CO2 | (3) |
| 2M3O4 + C → 6MO + CO2 | (4) |
| Li2O + CO2 → Li2CO3 | (5) |
| 2MO + C → 2M + CO2 | (6) |
The calcinated powder then undergoes water leaching to dissolve the lithium (Li2CO3) in the water. The metal oxide does not dissolve in the water. After water leaching via filtration, the undissolved metal oxide and the aqueous solution were separated to produce a Li2CO3 solution, followed by water evaporation to finally obtain Li2CO3 (Fig. 7). This method can process large numbers of disposed lithium-ion batteries, and the process is simple. Li et al. recycled lithium via pyrometallurgy using LiCoO2 and graphite from a pre-treated lithium-ion battery.67 The separated active materials were calcined in nitrogen at 1000 °C for 30 min to obtain Co, Li2CO3, and graphite compounds. This compound was submerged in water to separate lithium using wet magnetic separation. Pindar et al. separated lithium-ion batteries and calcinated them at 800 °C for 45 min to create a lithium-containing powder, which was dissolved in a mass of water 50 times more than the powder mass.72 This resulted in Li2CO3 with LiF mixed at a 90% lithium retrieval rate. Xiao et al. used pyrometallurgy to separate lithium from LiMn2O4, LiCoO2, and LiMnxCoyNizO2 mixed with graphite. The cathode material was separated from the battery and calcinated at 700 °C in vacuum for 30 min. The calcinated powder was a metal oxide, Li2CO3, which was then reacted with water (25 g L−1) for separation.68
![]() | ||
| Fig. 7 Overall schematic of lithium recycling from pre-treated waste LIB components by pyrometallurgy process. | ||
Some pyrometallurgy uses additional acids for the roasting to higher the lithium extraction efficiency. Liu et al. used nitric acid to nitrate the lithium ion-battery scraps and roasted them at 250 °C for 60 min. After roasting, by leaching with water, lithium solution was produced and with carbonation, Li2CO3 was produced with low-temperature roasting.73 Li et al. used sulfation roasting to recycle Li2SO4 from NCM523 material by using H2SO4 with the process of roasting and water leaching.76
Chlorination roasting is also used in pyrometallurgy, which uses sintered lithium slag (xLi2O·yCaO·zAl2O3·nSiO2) with chlorine donor to form LiCl after the roasting. Chang et al. used CaCl2 and roasted it at 1000 °C for 90 min with LiAl(SiO3)2 to transform it into LiCl71 (eqn (7)).
| CaCl2 + Li2O → CaO + 2LiCl | (7) |
The biggest drawback of the pyrometallurgy method for lithium recycling is that additional steps are required after calcination. This additional process usually involves dissolving the product in water or solvent and separating it.
However, the low solubility of Li2CO3 (13 g L−1) requires a large amount of solvent. In addition, the pyrometallurgy method requires complicated calcination equipment and can cause the emission of harmful gases. Table 4 summarizes the details of the pyrometallurgy research.
| Spent materials | Residue | Efficiency | Purity | Condition | Ref. |
|---|---|---|---|---|---|
| Electrode materials | Li concentrate | >90% | >99% | • 1700 °C–1750 °C | 66 |
| LiCoO2 + C | Co + Li2CO3 + C | 98.93% | — | • 1000 °C/30 min in O2 free | 67 |
| C + LiMn2O4, LiCoO2, LiMnxCoyNizO2 | Li2CO3 + metal oxide | 81.90% | 99.7% | • 700 °C/30 min | 68 |
| LiMn2O4 + C | Li2CO3 + MnO | 91.3% | 99.7% | • 800 °C/45 min | 69 |
| Cathode materials | Li2CO3 | 84.7% | — | • 650 °C/3 h | 70 |
| • Water leaching [100 °C/0.5 h] | |||||
| LIB lithium slag | LiCl | Evaporate 97.45% | — | • 1200 °C/1 h | 71 |
| • 1000 °C/90 min with CaCl2 | |||||
| Cathode materials | Li2CO3 solution | >90% | — | • 800 °C/45 min | 72 |
| LIB scraps | Li2CO3 | 90% | 99.95% | • 70 °C/5 h HNO3 | 73 |
| • Roasting 100–300 °C | |||||
| LiCoO2 | Li2CO3 solution | 36% | — | • 700 °C with carbon | 74 |
| Electrode materials | Li2CO3 | 80% | 98% | • Carbothermal 850 °C/45 min | 75 |
![]() | ||
| Fig. 8 Overall schematic of lithium recycling from pre-treated waste LIB components by hydrometallurgy process. | ||
These precipitation methods are most researched, but fine control of the operating conditions (pH, Li concentration, and temperature) is needed to produce the required property profile.
Generally, the hydrometallurgy method guarantees high recovery rates and does not require additional equipment, making it quite popular in the laboratory and the method closest to commercialization. However, this method requires a high volume of acid and base for leaching (proportional to the lithium-ion battery), which can incur additional chemical costs. In addition, the backend costs of disposing the used solutions can be high. Table 5 shows different hydrometallurgy methods, lithium extraction conditions, and results, with a focus on studies that resulted in the production of the final compound after leaching.
| Spent materials | Method | Residue | Efficiency | Purity | Condition | Ref. |
|---|---|---|---|---|---|---|
| LiCoO2 | Precipitation | Li2SO4 | 90% | — | • 4 M H2SO4, H2O2 [80 °C/4 h] | 77 |
| • Ethanol, LiOH | ||||||
| LIB scraps | Precipitation | LiF | 50% | >99 wt% | • 500 °C/5 h, KHSO4 | 78 |
| • 9 M H2SO4, 30 wt% H2O2 (3 mL g−1) [90–100 °C] | ||||||
| • 6 M NaOH | ||||||
| Cathode materials | Precipitation | Li2CO3 | 80 ± 1% | 96.97% | • 4 M HCl, [80 °C] (20 g L−1) | 79 |
| • Na2CO3 [100 °C] | ||||||
| Cathode materials | Precipitation | Li2CO3 | 71% | — | • 2 M H2SO4, 2% H2O2 (33g L−1) [60 °C] | 80 |
| • Na2CO3 [50 °C] | ||||||
| Mixed cathode materials | Precipitation | Li2CO3 | 80% | — | • 4 M H2SO4, 30 wt% H2O2 (50 g L−1) [70–80 °C] | 81 |
| • NaOH, Na2CO3 [40 °C] | ||||||
| LiNi0.3Mn0.3Co0.3O2 | Precipitation | Li2CO3 | Leaching 99.7% | — | • 3.0 M trichloroacetic acid, 4.0 vol% H2O (50 g L−1) [70–80 °C] | 82 |
| • Saturated Na2CO3 solution | ||||||
| Cathode materials | Precipitation | Li3PO4 | 89% | — | • Citric acid + H2O2 | 83 |
| • C4H8N2O2, (NH4)2C2O4, D2EHPA [55 °C] | ||||||
| • 0.5 M Na2PO4 | ||||||
| LiNi0.3Mn0.3Co0.3O2 | Precipitation | Li2CO3 | 98.22% | 99.9% | • 2 M formic acid, 2 vol% H2O2 (50 g L−1) [70 °C] | 84 |
| • Saturated Na2CO3 [20–60 °C] | ||||||
| LiFePO4 | Precipitation | Li3PO4 | 82.55% | 96.5% | • Ball mill with EDTA–2Na, 0.6 M H3PO4 (50 g L−1) | 85 |
| Cathode material + graphite | Precipitation | Li2CO3 | Leaching 99.9% | 99.4% | • 3 M acetic acid, 7.5%vol H2O2 (20 g L−1) [70 °C/40 min] | 86 |
| • Saturated Na2CO3 | ||||||
| LiFePO4 | Precipitation | Li2CO3 | 95.05% | 99.95 wt% | • 0.8 M CH3COOH, 6 vol% H2O2 (120 g L−1) [50 °C/30 min] | 87 |
| • Saturated Na2CO3 [95 °C] | ||||||
| Cathode materials | Precipitation | Li2CO3 | >90% | 99.93% | • 3.5 M acetic acid (40 g L−1), H2O2 4vol% [60 °C] | 88 |
| • Saturated Na2CO3 [20–60 °C] | ||||||
| Cathode materials | Precipitation | Li3PO4 | 85.56% | — | • Oxidation at 600 °C, 0.28 M H2SO4 + H2O2 (16 g L−1) [85 °C/2 h] | 89 |
| • NaOH, Na3PO4 | ||||||
| Anode | Precipitation | Li2CO3 | Leaching ≈ 100% | >99% | • 1.5 M HCl (100 g L−1) | 91 |
| • CO2 | ||||||
| LiNi0.3Mn0.3Co0.3O2 | Precipitation | Li2CO3 | Leaching 99% | — | • 2 M H2SO4 + 4 vol% H202 (50g L−1) [50 °C/2 h] | 90 |
| • KMnO4, C4H8N2O2 | ||||||
| • Na2CO3 [90 °C] | ||||||
| LiNi0.5Mn0.3Co0.2O2 | Precipitation | Li2CO3 | 76% | >99.5% | • 1 M of oxalic acid (10g L−1) [95 °C/12 h] | 92 |
| • 5 M K2CO3 [80 °C/4 h] | ||||||
| LiFePO4 | Precipitation | Li2CO3 | 99.35% | — | • Ball mill with citric acid, H2O2 (20 g g−1) | 93 |
| • Saturated Na2CO3 [95 °C] | ||||||
| Cathode | Precipitation | Li2CO3 | 38% | 99.48% | • 1 M H2SO4, 5 vol% H2O2 [60 °C/1 h], sonication | 94 |
| • 2 M NaOH | ||||||
| LiFePO4 | Precipitation | Li2CO3 | 80% | — | • 4 M MSA acid (80 g L−1) 18%, H2O2 | 95 |
| • 5% NaOH solution, 30% Na2CO3 [96 °C/30 min] | ||||||
| LiNi0.5Co0.2Mn0.3O2 | Precipitation | Li2CO3 | 91.23% | 99% | • Sodium persulfate (400 g L−1) [85 °C] | 96 |
| • Na2CO3 | ||||||
| LiNixMnyCo1−x−yO2 | Precipitation | Li3PO4 | Leaching 99.1% | — | • 750 °C/3 h, 2.75 M H3PO4 [40 °C/10 min] | 97 |
| • 10 M NaOH | ||||||
| LIB scraps | Solvent extraction | Li2CO3 | 80% | >98% | • 4 M H2SO4 (100 g L−1) glucose [90 °C] | 99 |
| • D2HEPA, CYANEX 272, saturated Na2CO3 | ||||||
| LiCoO2 | Solvent extraction | Li2SO4 Solution | Leaching 100% | >99.5% | • 600 °C/2 h, 2.25 M H2SO4 [80 °C/30 min] | 71 |
| • PC88A | ||||||
| LiNi0.3Mn0.3Co0.3O2 | Solvent extraction | Li2CO3 | Leaching 94% | — | • 2 M H2SO4 H2O2 (33 g L−1) [70 °C] | 100 |
| • Cyanex 272 | ||||||
| • Saturated Na2CO3 | ||||||
| LIB scraps | Solvent extraction | Li2CO3 | 72% | 99.7% | • H2SO4–H2O2 mixture | 101 |
| • NaOH, D2EHPA, Cyanex 272, kerosene, Na2CO3 [95 °C] | ||||||
| LiCoO2 | Solvent extraction | Li2CO3 | 86.2% | 74.2% | • 0.5 M HCl [60 °C] | 102 |
| • Cyphos IL-101, saturated Na2CO3 [60 °C] | ||||||
| LiNi0.5Co0.2Mn0.3O2 | Selective adsorption | Li2CO3 | Leaching 81.2% | >99.5% | • NH3·H2O (367.5 g L−1) + NH4HCO3 (140 g L−1) + H2O2 (63.24 g L−1) [manganese type lithium ion-sieves | 103 |
| • 0.5 M HCl leaching (10 g L−1) | ||||||
| • NaOH, Na2CO3 |
| 2LiOH → 2Li+ + 2e− + 1/2O2 + H2O | (8) |
The undissolved Li+ in the cathode powder can be separated by the same reaction as that of delithiation in the cathode material (eqn (9) and (10))
| LiMO2 → Li+ + e− + MO2 (M = Co, Mn, Ni) | (9) |
| LiFePO4 → Li+ + e− + FePO4 | (10) |
The charging potential differs depending on the type of cathode material in the waste. When the active material is placed in water, the aqueous solution becomes a strong base owing to the influence of LiOH. The OER reaction during charging differs in operating voltage depending on the pH, and in strongly basic conditions (pH > 11), the OER reaction occurs below 3.6 V.104 In the case of the LiFePO4 cathode powder, the delithiation reaction potential is 3.5 V, which is lower than the voltage of the OER reaction in the strong base, and Li+ is directly extracted from the cathode powder. However, for LiCoO2 (3.9 V), LiMn2O4 (4.0 V), and LiNi0.3Mn0.3Co0.3O2 (3.7 V), because the delithiation potential is higher than that of the strong base OER reaction, Li+ extraction from the solution occurs first, rather than from the cathode powder. However, during charging, the pH of the aqueous solution decreases because of the characteristics of the OER reaction, and the operating voltage of the OER reaction gradually increases. When the potential of the OER reaction exceeds that of the cathode powder material, Li+ extraction from the powder becomes possible. Through this OER reaction and the reaction for each cathode material, Li+ can be extracted and separated from both solution and powder, and when Li+ can no longer be extracted, the charging of the system is automatically completed.
After charging, the separated Li+ is discharged to water, passes through another ceramic solid electrolyte, and undergoes an oxygen reduction reaction (ORR) with water and electrons to form an aqueous LiOH solution. LiOH is a strong base that is used for CO2 capture because it is highly reactive with CO2 forming Li2CO3 (Fig. 9). The formation of Li2CO3 can be expressed as follows (eqn (11) and (12)):
| 2Li+ + 2e− + 1/2O2 + H2O → 2LiOH | (11) |
| 2LiOH + 2CO2 → 2Li2CO3 + H2O | (12) |
![]() | ||
| Fig. 9 Overall schematic of lithium recycling from pre-treated waste LIB components by electrochemical extraction process. | ||
Electrochemical extraction is a technology that can afford Li2CO3 powder without the need for drying or precipitation. When the system is continuously discharged, Li2CO3 powder precipitates naturally. When discharge occurs, the concentration of Li+ in the water increases gradually, followed by an increase in the concentration of Li2CO3. In addition, owing to the ORR, H2O is consumed and the concentration of Li2CO3 increases relative to the decrease in the quantity of the solvent. This leads to the natural precipitation of Li2CO3.
An electrochemical system was developed to separate lithium from the cathode, anode, and electrolyte from a discarded lithium-ion battery.105 This device uses a Li1+x+yTi2−xAlxP3−ySiyO12 solid electrolyte that transmits lithium selectively and has physically separated liquid cathode and anode parts. The liquid cathode contained LiFePO4, LixC6, and 1 M LiPF6-EC:DMC. Through electrochemical charging, lithium is separated and passed through the solid electrolyte to separate the lithium metal from the anode. In later studies, an advanced system was developed to separate lithium from LiFePO4, LiMn2O4, and LiNi0.3Mn0.3Co0.3O2 cathode powders.106 This system is composed of a waste cathode, harvesting anode, and recycling cathode, and each compartment is physically separated by a solid electrolyte. In the actual electrochemical system, a polymer film was used as the body of the system, solid electrolytes were attached to both sides, and an anode was placed in the middle to produce a harvesting anode. A harvesting anode was inserted between the waste cathode and recycling cathode to separate the battery into three compartments (Fig. 10a). The fabricated electrochemical lithium extraction system can extract lithium through electrochemical charging and discharging, as shown in Fig. 10b. The cathode powder from the lithium-ion battery contacted the waste cathode current collector of the waste cathode. During electrochemical charging, Li+ extraction from the cathode powder occurs, passing through the solid electrolyte, followed by an electrochemical reaction at the harvesting anode to form metallic lithium (Fig. 10c). By discharging the separated lithium from the harvesting anode to the distilled water, Li2CO3 can be formed via a reaction with water, oxygen, and CO2 (Fig. 10c). Actual discarded lithium-ion batteries were tested using this system and it was proved that Li2CO3 can be recycled.
The electrochemical extraction method can extract 75–95% of lithium from active material powder during recycling, and it can extract not only Li2CO3 compounds but also lithium metal if necessary. The recycled lithium metal was analyzed using inductively coupled plasma analysis and showed a purity of 99%. In an additional experiment, the purity of the final material, Li2CO3, was analyzed via the acid–base titration method (Standardization Administration of the People's Republic of China (SAC) method), and the purity was 99.6%.
This method only requires charging and discharging and does not require additional chemical compounds or an increase in temperature. With this system, lithium-ion batteries can be recycled in an environment-friendly manner using only water. In addition, by using a special solid electrolyte that allows only lithium to pass through, high-purity lithium can be separated and be used as an energy storage system. However, this method requires the setting up of an electrochemical system and solid electrolyte and has only been proven on a laboratory scale; further research is required before it can be scaled up for commercialization. Table 6 lists the research methods using electrochemical extraction. To scale up the system, research is being conducting to increase the efficiency and speed of Li extraction by designing a cell structure, expanding the area of the solid electrolyte and stacking the system. In addition, since this electrochemical lithium extraction method can extract lithium from LiOH, as well as other lithium solutions in any form, studies are being conducted not only on Li-ion batteries but also on Li-containing glasses.
Three methods to produce lithium compounds from a pre-treated lithium-ion battery have been discussed: pyrometallurgy, hydrometallurgy, and electrochemical extraction. These techniques are still under research, and the methods can be combined to overcome their respective drawbacks.
Table 7 lists quantitative metrics on the pyrometallurgy, hydrometallurgy, and electrochemical lithium recycling methods. These metrics include the recycling efficiency, additional cost of chemicals, operating temperature, complexity, pollutant production, and commercialization level. The methods only consider the lithium extraction process after pre-treatment, as the pre-treatment methods can vary depending on the lithium-ion battery type and quantity. The lithium recycling efficiency and purity is obtained from available literature regarding the methods. For the additional cost of chemicals, the price was normalized per kilogram of discarded active material powder, after considering the required amount and price.107–109 Operating temperature considers the temperature range needed for lithium extraction. For complexity, the essential steps for each method are examined. Pollutants include different polluting materials that can result from each recycling process, and the level of commercialization separates the methods that already have been commercialized and methods that are only developed at a laboratory level.
| Li recycling method | Recycle efficiency (%) | Purity (%) | Additional chemical cost ($ kg−1) | Temperature (°C) | Complexity | Potential pollutions | Commercial readiness |
|---|---|---|---|---|---|---|---|
| Pyrometallurgy | 80–98.9 | 98–99.95 | 1.894 m−3 (flowing gas (N2), depends on furnace size) | 650–1700 | 2 Steps | Volatile organic compounds | Commercialized [Accurec GmbH] |
| • Oxygen free roasting | |||||||
| • Wet magnetic separation | |||||||
| Hydrometallurgy [precipitation] | 76–98.2 | 96.5–99.97 | 3.18 (CH2O2, H2O2etc.) | 50–100 | 3 Steps | Inorganic waste | Commercialized [TOXCO (Retriev)] |
| • Leaching | Acidic waste | ||||||
| • Other metal precipitation (pH adjustment) | |||||||
| • Li precipitation | |||||||
| Hydrometallurgy [solvent extraction] | 72–86.2 | 74.2–99.7 | 73.3 (H2SO4, PC88A etc.) | 60–90 | 4 Steps | Inorganic waste | On research |
| • Leaching | Organic waste | ||||||
| • Solvent extraction | Acidic waste | ||||||
| • Solution separation | |||||||
| • Precipitation | |||||||
| Hydrometallurgy [selective adsorption | Leaching 81.2 | >99.5 | 14.9 (NH3, HCl etc. | 30 | 4 Steps | Acidic waste | On research |
| • Leaching | |||||||
| • Sieve adsorption | |||||||
| • Sieve leaching | |||||||
| • Precipitation | |||||||
| Electrochemical extraction | 75–92 | >99 (metal) | — | Room temp. | 2 Steps | — | On research |
| • Charging | |||||||
| • Discharging |
Fig. 11 is based on Table 7 and describes the characteristics of each method using a spider plot. The image shows the relative magnitudes of the different metrics involved in lithium extraction.
![]() | ||
| Fig. 11 Performance and industrial comparisons of lithium recycling technologies from waste LIBs, pyrometallurgy, hydrometallurgy and electrochemical extraction. | ||
Accurec pre-treats the battery mechanically to separate the plastic, followed by vacuum thermal treatment to remove the electrolyte and solvent. The material is then crushed, sieved, and separated (magnetically and with air) to separate Al, Fe, Cu, and plastic. The pre-treated material then undergoes pyrometallurgy treatments, namely, reduction to separate Co and Mn, followed by hydrometallurgy and acid leaching to precipitate LiCl.112
Retriev's pre-treatment processes include the use of liquid nitrogen in the cryo-milling process (at −196 °C) followed by the use of a hammer mill to crush the material. Subsequently, Cu, Co, and Al were separated on a shaker table, and the remaining cathode and anode material were processed in a filter tank and carbon filter press to remove the metal oxide and carbon. Na2CO3 was added to the solution to precipitate Li2CO3.113,114
The last decade has seen a global rise in the interest in lithium recycling. However, issues remain regarding the means to commercialize and make the process more environmentally friendly. According to the UNEP report on recycling rates, the lithium-ion battery recycling rate in the EU is less than 5%, and less than 1% of lithium is recycled.115–118
![]() | ||
| Fig. 12 Future requirements for waste LIB recycling: recycling from various lithium sources, safe treatment, eco-friendly recycling, economical recycling. | ||
(1) Although the increase in the demand for lithium is due to lithium-ion batteries, technological development to extract lithium from other products is needed. There is almost no research on the extraction of lithium from non-batteries. Because 35% of the lithium is used for glass, grease, and casting (as of 2019), more attention should be paid to the recycling of lithium from these products. The best option could be to leverage the technologies developed for recycling lithium-ion batteries to extract lithium from other waste lithium sources. Overall, this positively affects the entire lithium cycle.
(2) Even if lithium materials are collected for recycling in an organized manner, it is difficult to process them simultaneously. For batteries, the materials for the cathode, anode, and electrolytes, as well as the size of the batteries, vary widely. Processing them simultaneously holds the risk of problems such as explosions. A policy is needed to categorize or automatically process the disposed lithium material. In addition, it is important to pre-treat lithium-containing materials to increase the efficiency of lithium recycling. With a safe and environmentally friendly pre-treatment method, considerable quantities of lithium materials can be processed to significantly increase the speed of the lithium cycle.
(3) Currently, the techniques that are widely commercialized or researched are also environmentally harmful. Lithium recycling technology should not only mitigate lithium scarcity but also reduce waste to prevent environmental pollution. However, most currently developed recycling methods produce pollutants. This includes harmful gases created by the heat treatment of lithium waste and the acids, bases, and organic solvents used for leaching. This also leads to additional expenses. The extra costs and procedures can hinder the commercialization of the process. Thus, substantial consideration should be given to streamlining the process to minimize waste products or finding ways to reuse the waste products from these processes.
(4) For such a process, economics cannot be ignored. If the purchasing cost is lower than the recycling cost, recycling would not be economically appropriate or viable. Current methods that use acids or bases or operate at high temperatures are usually costly and energy-intensive. The involvement of more chemicals in the process will increase the cost of the process. The quantities of acids and bases required for lithium recycling are substantially greater than that of the recycled product, which is economically disadvantageous. Thus, methods to reuse the acids and bases, or to lower the operating temperature, must be developed to minimize the cost and energy required to recycle lithium. If an economically viable method emerges, this will accelerate interest in the development of lithium recycling technologies.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ma00216c |
| This journal is © The Royal Society of Chemistry 2021 |