Jiawen
Liu
a,
Jiahui
Lin
a,
Kai
Yi
a,
Fangyan
Liu
b,
Feng
Gao
a,
Mengye
Wang
*a and
Feng
Huang
ac
aState Key Laboratory of Optoelectronic Materials and Technologies, School of Materials, Sun Yat-Sen University, Guangzhou, 510275, China. E-mail: wangmengye@mail.sysu.edu.cn
bState Key Laboratory of Optoelectronic Materials and Technologies, Guangdong Province Key Laboratory of Display Material and Technology, School of Electronics and Information Technology, Sun Yat-Sen University, Guangzhou, 510275, China
cGanjiang Innovation Academy, Chinese Academy of Sciences, Ganzhou, 341000, China
First published on 29th February 2024
With the increasing severity of antibiotic pollution, the development of effective green photocatalysts for the degradation of organic pollutants in water has attracted extensive attention. Herein, we have prepared CuO/C3N4 S-scheme heterogeneous photocatalysts via recycling Cu resources from Cu-containing electroplating sludges. By mediating the acid leaching process, copper in electroplating sludges was dissolved selectively, while other metal species were retained in the residues. The CuO/C3N4 S-scheme heterojunction not only effectively suppressed the recombination of photogenerated charge carriers of C3N4, but also preserved the strong reducing electrons of C3N4 and the strong oxidizing holes of CuO, retaining the outstanding redox ability of CuO/C3N4. Therefore, CuO/C3N4 photocatalysts exhibited good catalytic performance in the degradation of tetracycline (over 95% in 2 h). In addition, CuO/C3N4 S-scheme heterojunctions achieved a high mineralization rate (45% in 2 hours), thus reducing secondary pollution during the degradation. This work provides a reliable direction for designing novel S-scheme heterojunction photocatalytic materials by using metal sources in solid waste.
As the key to photocatalytic degradation, the issue of how to improve the separation efficiency of photogenerated carriers needs to be urgently resolved.17–22 To solve this problem, it is a common method to construct heterojunctions. However, in the conventional type II heterojunction structure, the carrier separation efficiency is improved at the expense of the redox capacity of the catalyst.23 By forming an internal electric field between an oxidation catalyst and a reduction catalyst, the S-scheme heterojunction can not only ensure the effective carrier separation of both catalysts, but also improve their redox capability.24–26 Among the common photocatalysts, C3N4 has garnered significant attention due to its narrow band gap, suitability for visible light absorption, facile synthesis, excellent thermal stability, and robust acid and alkaline resistance.27–32 Although the narrow band gap of C3N4 brings a good visible light absorption capacity, it restricts the redox capacity of C3N4. In addition, pure-phase C3N4 also exhibits drawbacks in photocatalysis, such as high carrier recombination rate.33,34 By combining C3N4 with CuO with its more positive valence band to form an S-scheme heterojunction, the carrier separation efficiency and redox ability of C3N4 can be intensively improved.
As one of the indispensable metals in our daily life, copper products are widely used in all walks of life. However, the extensive use of copper products has resulted in large amounts of copper-containing solid waste.35 Considering prevailing resource scarcity, these solid waste materials represent misallocated reserves of accessible metal resources.36,37 In our work, a simple approach was employed to extract copper from solid waste through acid leaching and integrate it with C3N4 to fabricate CuO/C3N4 composite heterojunction materials. Considering that both CuO and C3N4 are n-type semiconductors with significant difference in electronic band positions, a novel S-scheme heterojunction could be constructed. The formation of the S-scheme heterojunction was verified through the characterization of Mott–Schottky curves and band structures. Due to the electrons in C3N4 at the high Fermi level drifting to CuO at the low Fermi level, the C3N4 interface became positively charged and the CuO interface became negatively charged, creating an internal electric field directed from CuO to C3N4. At the same time, the energy bands at the C3N4 and CuO interfaces were also bent upward and downward, respectively. This band bending and the formation of the internal electric field effectively inhibited carrier recombination and increased carrier lifetime from 1.32 ns to 4 ns. In addition, strong reducing electrons and oxidizing holes were retained in the conduction band of C3N4 and the valence band of CuO, respectively, which preserved the strong redox ability of CuO/C3N4. After a photocatalytic reaction for 2 h, the degradation rate of tetracycline exceeded 95%, and its mineralization rate approached 50%. These results confirmed the significant photocatalytic performance of the CuO/C3N4 materials.
Fig. 1 (a) XRD pattern of the sludge. (b) Pie chart of the elemental distribution of the sludge. (c) Schematic illustration of the synthetic process of CuO/C3N4. |
To investigate the morphology of copper oxide and C3N4, further characterization of CuO/C3N4-2 was conducted using transmission electron microscopy (TEM). TEM images provided direct visualization of the two-dimensional nanosheet structure of C3N4 (Fig. 2a). In Fig. 2b, the lattice spacing values of 0.25 nm and 0.33 nm can be observed, belonging to the (111) crystal plane of CuO and the (002) crystal plane of C3N4, respectively. This confirmed that the copper species were loaded onto C3N4 in the form of copper oxide after the calcination process and formed a heterogeneous interface. Cu and O elements were concentrated within the particle clusters, while C and N elements were uniformly distributed throughout the nanosheet structure. In Fig. 2f, it was observed that oxygen element also existed in the C3N4 sheet area. Considering that the macromolecular precursor was calcined under an air atmosphere, oxygen element was inevitably doped into the C3N4 lattice. Some studies have shown that oxygen doping could effectively regulate the electron state density and band structure of C3N4 and improve the catalytic efficiency.38,39 This spatial distribution of elements provided additional evidence supporting the presence of CuO in the form of clusters on the surface of the C3N4 sheet.
Fig. 2 (a) TEM image and (b) HRTEM image of CuO/C3N4-2. EDS elemental distribution mappings of (c) C, (d) N, (e) Cu and (f) O of CuO/C3N4-2. |
In order to further explore the composition and phase structure of the as-synthesized samples, X-ray diffraction (XRD) patterns and Fourier transform infrared (FTIR) spectroscopy measurements were conducted. Pure C3N4 exhibited diffraction peaks at 12.8° and 27.5°, agreeing well with the (100) and (002) crystal planes of C3N4, respectively (Fig. 3a). Different proportions of CuO/C3N4 catalysts were prepared by changing the calcination amount of the macromolecular polymer precursors. From CuO/C3N4-1 to CuO/C3N4-3, the increasing intensity of peaks at 35.2° and 38.6° attributed to the (1−11) and (111) crystal planes of CuO, respectively, indicated that the content of CuO increased gradually. In Fig. 3b, IR signals at 815 cm−1, 1150–1700 cm−1, and 3000–3400 cm−1 were attributed to the structural bending of tri-s-triazine units, stretching vibration modes of C–N heterocycles and N–H stretching of the amino groups, respectively (Fig. 3b). Compared with pure C3N4, CuO/C3N4 showed no obvious change, indicating that the structure of C3N4 remained unchanged despite the modification of CuO.
The absorption capacity of visible light plays a crucial role in the photocatalytic performance of a photocatalytic material. To investigate the influence of copper oxide on the absorption capacity of C3N4, UV-vis absorption spectra were recorded. Compared with pure C3N4, CuO/C3N4-2 demonstrated a noticeable red shift in the absorption edge after the introduction of CuO. This observation indicated that the formation of a CuO/C3N4 heterojunction effectively broadened the wavelength range of light utilized by the catalyst. Moreover, the absorption intensity of the catalyst in the visible range was significantly enhanced in comparison with pure C3N4. This finding confirmed that the introduction of CuO contributed to the improvement of photon utilization efficiency of C3N4 during the photocatalytic process, leading to an enhanced overall photocatalytic performance of C3N4. By employing the Kubelka–Munk equation, the band gaps of pure C3N4 and CuO/C3N4-2 catalysts were calculated to be 2.98 eV and 2.90 eV, respectively. CuO loading thus reduced the band gap of C3N4 by approximately 0.08 eV. Moreover, the VB-XPS spectra of C3N4 and CuO are shown in Fig. 3d. These suggested that the VB was 2.38 eV and 1.71 eV for CuO and C3N4, respectively.
To investigate the chemical states of pure C3N4 and CuO/C3N4-2, X-ray photoelectron spectroscopy (XPS) was employed. Compared with pure C3N4, CuO/C3N4-2 exhibited additional binding energy peaks around 940 eV (Fig. 4a), which can be attributed to the presence of copper. High-resolution Cu2p XPS spectra of CuO/C3N4-2 are shown in Fig. 4b. The peaks at 951.8 eV and 932.0 eV were assigned to Cu2+2p1/2 and Cu2+2p3/2, respectively. The apparent satellite peaks at 961.7 eV and 941.9 eV in Fig. 4b indicate that the copper species was copper oxide rather than elemental copper or cuprous oxide. The high-resolution XPS spectra of N1s reveal peaks at 397.5 eV, 398.9 eV, and 400.1 eV, corresponding to nitrogen bonded in C–NC in sp2 hybridization, the N–C3 bond in sp3 hybridization, and the amino C–N–H bond in sp3 hybridization, respectively (Fig. 4c). The ratio of sp2 hybridized nitrogen to sp3 hybridized nitrogen was calculated for the C3N4 and CuO/C3N4 samples, and it was 2.45 and 1.53, respectively. These findings suggested that the incorporation of copper species partly occupied the position of sp2-hybridized nitrogen of C3N4, leading to a decrease in the content of sp2-hybridized nitrogen. Additionally, the N/C atom ratio decreased from 0.75 to 0.6 upon the modification of copper oxide, indicating the emergence of nitrogen vacancies in the sp2 hybrid nitrogen sites.
Fig. 4 (a) XPS survey spectra of pure C3N4 and CuO/C3N4-2. (b) High-resolution Cu2p XPS spectra of CuO/C3N4-2. High-resolution XPS spectra of (c) N1s and (d) C1s of pure C3N4 and CuO/C3N4-2. |
Fig. 4d displays the high-resolution XPS spectra of C1s. The peaks at 283.8 eV, 285.1 eV, and 287.1 eV were in agreement with graphitized carbon, the C–NH2 bond, and sp2 hybrid carbon, respectively. In comparison with C3N4, the proportion and position of carbon atoms connected to the amino group in CuO/C3N4 samples were significantly changed, indicating a strong interaction between copper oxide and C–NH2. The ratio of sp2 hybrid carbon to sp3 hybrid carbon decreased from 1.61 to 1.03, which aligned with the change trend observed in the N/C atom ratio. This further confirmed the influence of copper oxide loading on the chemical environment of carbon and nitrogen elements of C3N4. Moreover, the presence of C–NC structures in the N1s spectra and N–CN structures in the C1s spectra demonstrated the existence of the tri-s-triazine ring structure in the sample.
To evaluate photogenerated carrier separation and transmission efficiency of pure C3N4 and CuO/C3N4, photocurrent measurements, electrochemical impedance spectroscopy (EIS), steady-state photoluminescence (PL) spectroscopy and time-resolved photoluminescence (TRPL) spectroscopy were conducted, as depicted in Fig. 5. The photocurrent generated by CuO/C3N4-2 (about 0.4 μA cm−2) under xenon lamp illumination was 2.6 times greater than that of pure C3N4 (about 0.15 μA cm−2, Fig. 5a). The photocurrent generated by CuO/C3N4-1 and CuO/C3N4-3 under the same xenon lamp was 0.28 μA cm−2 and 0.32 μA cm−2, respectively. These results indicated that the introduction of CuO significantly enhanced the separation efficiency of photogenerated electrons and holes. The EIS spectra showed that the electrochemical impedance of CuO/C3N4-2, CuO/C3N4-3, CuO/C3N4-1 and pure C3N4 increased gradually (Fig. 5b). This suggested that the charge transfer ability at the interface between CuO/C3N4 and solution was substantially higher than that between pure C3N4 and solution, ultimately improving the photocatalytic efficiency. The fluorescence intensity of CuO/C3N4 was considerably lower than that of pure C3N4 (Fig. 5c). This indicated that the introduction of CuO effectively suppressed the recombination of photogenerated electrons and holes, leading to enhanced visible light utilization efficiency. By employing double exponential function fitting, the average lifetimes of pure C3N4 and CuO/C3N4-2 were calculated to be 1.32 ns and 4.00 ns, respectively. The average lifetime of CuO/C3N4-2 was approximately three times greater than that of pure C3N4, indicating that CuO decoration significantly decreased the recombination rate of photo-induced charge carriers.
Fig. 5 (a) Photocurrent responses, (b) EIS spectra and (c) PL spectra of pure C3N4, CuO/C3N4-2, CuO/C3N4-2 and CuO/C3N4-3. (d) TRPL spectra of pure C3N4 and CuO/C3N4-2. |
To investigate the effect of CuO modification on the photocatalytic performance of C3N4, tetracycline (TC) was utilized as the target pollutant for degradation under xenon lamp irradiation. Tetracycline has caused significant environmental harm due to its widespread misuse. For comparison, the same degradation tests were performed with commercial CuO. The degradation experiments were performed using a 30 mg L−1 tetracycline solution with 20 mg of catalysts under xenon lamp illumination, preceded by a 30-minute adsorption test in the dark. The results demonstrated that the degradation rate of TC can exceed 95% within 2 hours using CuO/C3N4 as the catalyst, whereas the degradation rates of pure C3N4 and CuO were only around 50% (Fig. 6a). This tremendous improvement in degradation efficiency using CuO/C3N4 as the catalyst was primarily attributed to the introduction of copper oxide. The presence of copper oxide enhanced carrier separation efficiency, increased visible light utilization, and reduced carrier recombination rates, thereby facilitating the improved photocatalytic efficiency. In Fig. S3,† it is shown that the degradation rate of the sample was over 90% after five cycles. This result indicated that our samples have good stability under catalytic reactions. It can be observed in Fig. S4† that the morphology of the CuO/C3N4-2 had no obvious change after 5 cycles. In addition, the peak position in the XRD pattern had no significant deviation, suggesting that our samples had good stability. By comparing three CuO/C3N4 catalysts, it was found that the photocatalytic degradation performance of CuO/C3N4-2 was better than those of CuO/C3N4-1 and CuO/C3N4-3. This was due to the low CuO content of CuO/C3N4-1, resulting in the limited formation of heterojunctions. Moreover, the high CuO content of CuO/C3N4-3 caused the agglomeration of CuO on the surface of C3N4, leading to its low photocatalytic activity.
In addition to degradation efficiency, the ability to mineralize tetracycline is an important parameter to evaluate the production of highly toxic intermediate products and secondary pollution during the degradation process. TC samples degraded by CuO/C3N4-2 were collected every half an hour, and the mineralization rate and total organic carbon (TOC) removal rate were measured. After two hours, the mineralization rate of tetracycline approached 50%, and the total organic carbon content decreased by 30% (Fig. 6b). In contrast, the mineralization rates of some other catalytic materials for the photodegradation of tetracycline are given in Table S1.† These results confirmed that the catalyst exhibited not only excellent degradation efficiency, but also good mineralization ability to decompose tetracycline, ensuring the transformation of the pollutant into less harmful byproducts.
In order to explore the mechanism of photocatalytic degradation of heterojunctions formed by CuO and C3N4, the schematic diagram of band structure was composed, as shown in Fig. 6c. To obtain the carrier concentrations of C3N4 and CuO, the Mott–Schottky curves were tested at 1 kHz, as shown in Fig. S5.† The slopes of the curves are both positive, indicating that C3N4 and CuO are n-type semiconductors. According to the Mott–Schottky equation, the carrier concentrations of C3N4 and CuO were 3.07 × 1014 cm−3 and 7.36 × 1012 cm−3, respectively. Based on the relationship between the carrier concentration and the Fermi level, such a carrier concentration caused the Fermi level of an n-type semiconductor to shift by about 0.1 eV towards the conduction band at room temperature.40 As the Fermi level of C3N4 was higher than that of CuO, an interfacial charge transfer occurred after contact between C3N4 and CuO. Electrons drifted from C3N4 to CuO. As a result, the C3N4 side lost electrons with positive charges, and the CuO side obtained electrons with negative charges, forming an interfacial electric field (IEF) and causing the band to bend. This resulted in a typical n–n S-scheme heterojunction structure consisting of a reduction photocatalyst (C3N4) with a higher Fermi level and an oxidation photocatalyst (CuO) with a lower Fermi level. This promoted the transfer of electrons from the conduction band of CuO to the valence band of C3N4. Compared with a conventional type II heterojunction, an n–n S-scheme heterojunction structure not only ensures the separation of photogenerated carriers, but also maintains the high redox capacity of the catalyst. Therefore, CuO/C3N4 catalysts that form S-scheme heterojunctions show both good TC degradation performance and good TC mineralization ability.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3nr06410g |
This journal is © The Royal Society of Chemistry 2024 |