Fabio A.
Pires
ab,
Gabriel T.
dos Santos
ac,
Jefferson
Bettini
a,
Carlos A. R.
Costa
a,
Renato V.
Gonçalves
d,
Ricardo H. R.
Castro
e and
Flavio L.
Souza
*abf
aBrazilian Nanotechnology National Laboratory (LNNano), Brazilian Center for Research in Energy and Materials (CNPEM), Campinas, SP, Brazil. E-mail: flavio.souza@lnnano.cnpem.br
bInstitute of Chemistry, State University of Campinas (UNICAMP), Campinas, SP, Brazil
cEngineering School, Federal University of Rio Grande do Sul (UFRGS), Porto Alegre, RS, Brazil
dSão Carlos Institute of Physics, University of São Paulo (USP), São Carlos, SP, Brazil
eDepartment of Materials Science and Engineering, Lehigh University, Bethlehem, PA 18015, USA
fCenter for Natural and Human Sciences, Federal University of ABC (UFABC), Santo André, SP, Brazil
First published on 7th September 2023
The design of nanostructured materials for photoelectrochemical water splitting relies on a detailed understanding of the reactional bottlenecks. For hematite, a model system for photoanodes, the challenges concern poor charge transfer and separation, carrier recombination rate, and sluggish water oxidation kinetics. Several methods have been proposed to address each individually, with complex multi-step processes offered as solutions to improve overall performance. Here, we introduce a single polymeric precursor solution that enables the design of hematite (α-Fe2O3) with synergistic bulk and interfacial engineering using Ga3+, Hf4+ and NiFeOx. The solution causes Ga3+ to dope hematite lattice to reduce polaronic effects, while simultaneously induces Hf4+ enrichment at both surface and grain boundaries, improving charge separation and reducing recombination. Hf4+ also led to a refined microstructure derived from interface stabilization, which associated with Ga3+ bulk doping and NiFeOx electrodeposition resulted in a thin film with 65% of overall photoelectrode efficiency. As a consequence, the modified hematite photoanode (176 nm-thick) delivered a water oxidation photocurrent of 2.30 mA cm−2 in contrast to 0.37 mA cm−2 for the pristine system measured at 1.23 V against hydrogen reversible electrode (RHE). The results suggest the simplicity of this new polymeric solution may offer a cost-effective, scalable and versatile alternative for multiple chemical modifications in oxides beyond hematite.
Over the years, record-breaking performances of hematite as photoanodes for solar water splitting have been associated with columnar morphology obtained by hydrothermal/solvothermal methods.4,5 The columnar structure mitigates common hematite deficiencies, such as poor hole (h+) diffusion length and electron–hole pair short lifetime.6,7 This contrasts with typical interface-rich microstructures obtained by sol–gel methods, which show poor efficiency due to a high concentration of recombination sites and low electronic conduction.8,9 However, the benefits of simple solution-based processes continued to inspire strategies to solve those intrinsic microstructural drawbacks to enable effective photoanode design.
More recently, homogeneous hematite nanostructured thin films were produced by a low-cost spin-coating deposition of a polymeric precursor solution.10,11 The produced films still presented limited photoelectrochemical performance,11 but the optimization of thermal treatments led to improved wettability and roughness for an incremental enhancement of photocurrent.12 Subsequently, a better understanding of the impact of annealing processes on electron trapping,13 the establishment of the performance dependence on dopant positioning (i.e., interface versus crystal lattice doping),13 and the practical benefits of solvent exchange to improve wettability,12 resulted in a paradigm-shifting on photoanode design, scilicet, from the morphology-centered to one focused on interfacial properties and dopant engineering to enable cost-effective production routes.14
The concept of dual (or multi) chemical modifications for mitigating efficiency-hindering features in hematite photoanodes has brought further performance improvement.15,16 For instance, tetravalent ions, such as Ti4+,17 Zr4+,18 Si4+,19 and Sn4+,20,21 commonly used in hematite as single modifiers have been employed in multi modification investigations22 combined with Be2+,23 Zn2+,24 Al3+,25 In3+,26 Nb5+,27 N3−,28 F−,29,30 among others, in the search for higher water oxidation photocurrents. However, the modifications increased the synthesis and device production complexity by demanding multi-step protocols to deliver each chemical change.29 Moreover, dopants are not necessarily synergistic or additive, and it is not uncommon to observe dopants weakening each other in multi-doping systems,31 requiring further study to augment the understanding of doping engineering.
Fundamentally, modification by dopants can be grouped based on their placement in the system. When the dopant is within the crystal lattice, i.e., the ions form solid solution with hematite in its corundum structure, the dopant affects donor density in response to charge balancing32 and may also minimize polaronic effects by structural stabilization.33 On the other hand, if ions preferentially segregate to interfaces, or in other words form interfacial excesses,34 the changes in the local chemistry may impact energy barriers between grains and grains-substrate for improved charge transport and, when located at the surface, impact the response of the system to gas phase chemistry.35,36 From a microstructural perspective, interface excess is also associated with the stability of nanostructures,37 as the excesses lead to local energy reductions, as described by the Gibbs adsorption isotherm.38 This interfacial energy reduction results in coarsening inhibition, for smaller grain sizes and greater thermal stability.34
In this work, we hypothesize that the design of a specific dopant placement can potentially mitigate dopant competitive behaviors to enable unprecedented photoanode efficiencies. Therefore, we introduce a solution process for the fabrication of synergistically engineered bulk (crystal lattice) and interface on hematite thin films. The process entails a hematite polymeric precursor containing trivalent modifying cations mixed with tetravalent ions added at different synthesis stages to form a single liquid precursor to be either spin coated, dip coated, or sprayed onto a conductive surface to build the components of a photoelectrochemical cell.
The proper dopant selection combined with the synthesis strategy allows for a predictive allocation of the dopants in the nanostructure. For demonstration, Ga3+ dopant was selected for hematite (crystal) because of its similarity in terms of valence, ionic radius size (Ga3+ = 62 pm; Fe3+ = 64) pm, and coordination number to Fe3+,39 theoretically benefiting solid solution formation.40 Targeting the interfacial chemical manipulation, Hf4+ was selected following segregation design strategies,34i.e., it shows ionic radius mismatch with both Ga3+ and Fe3+ (Hf4+ = 72 pm39), suggesting unfavorable formation of solid solution, while being unlikely to form a second phase in the concentrations and thermal treatment temperatures adopted.41
Targeting an enhancement on the surface charge transfer kinetics, NiFeOx oxygen evolution reaction (OER) catalyst was electrodeposited onto Ga–Hf-co-doped photoanode to reduce the overpotential for water oxidation.42 Nickel-iron alloys, such as hydroxides, oxyhydroxides and oxides are well-known non-noble metal alternatives with high stability and faradaic efficiency43 to modify hematite surface. The introduced modifications resulted in a remarkable performance enhancement for the hematite-based photoanodes, with an overall photoelectrode efficiency of 65% in the conversion of absorbed light into photocurrent density, which by itself demonstrates the success of the design strategies and open great perspectives for future technological developments.
Control solutions were previously prepared following the same steps to obtain (i) pristine hematite (H), (ii) Ga3+-modified (Ga0.1H, Ga0.5H and Ga1.0H) samples, and (iii) Hf4+-modified (HHf1.0, HHf2.0, HHf3.0, HHf4.0, HHf5.0, HHf6.0 and HHf7.0) samples. The optimal concentrations for the co-doped solution (0.5% Ga3+ and 3.0% Hf4+) were selected based on the responses of those control products.
All thin films were prepared on aluminium borosilicate glass (1.0 mm thick) substrates coated with fluorine-doped tin oxide (FTO, Solaronix, RΩ 8–10 Ω cm−1, >80% transmission from 500 to 800 nm, 2 cm × 1 cm). First, the substrates were cleaned by successive rinsing in acetone and ethanol for 30 min each at ∼70 °C and in Milli-Q water (18.2 MΩ cm) under ∼100 °C heat for 30 min. After, the substrates were thermally treated at 550 °C for 60 min (Lindberg/Blue M Mini-Mite horizontal tube furnace, model TF55035A). Then, 100.0 μL of polymeric solution was deposited onto the FTO surface with a spin-coating equipment (Laurell Tech. Corp., model WS-650MZ-23NPP) using 500 rpm for 5 s and 7000 rpm for 30 s. After coating, the thin films were thermally treated at 550 °C in air atmosphere for 30 min (Lindberg/Blue M Mini-Mite horizontal tube furnace, model TF55035A) and then at 750 °C in N2 flux (18 mL min−1) for 30 min (OTF-1200X-50-SL automatic sliding quartz tube furnace, MTI Corporation). Annealing under N2 flux was carried out by sealing the furnace tube to a coupled vacuum pump and pressure gauge. The quartz tube where the samples were placed underwent three consecutive steps of evacuation/pressurization with N2 gas, which flux was kept throughout the thermal treatment. After this step, the furnace was slide to the sample position and the thermal treatment started. The furnaces were preheated at employed temperatures and the region where the samples were placed had their temperatures verified by an external thermocouple. Temperatures and duration of thermal treatments adopted in this work were optimized as reported elsewhere44,45 to preserve the substrate integrity and conductivity. Fig. S1† shows a schematic visualization of all processes involved in the fabrication of the photoelectrodes.
Jabs = −qø(1 − e(−∫Absdy)) | (1) |
The optical band gap energies of the photoelectrodes were estimated from UV-vis absorption spectra according to the Tauc relation (eqn (2)), where α is the absorption coefficient, h is the Planck constant, ν is the frequency, n is ½ for allowed indirect electronic transitions and 2 for allowed direct transitions, A is a constant, and Eg is the estimated optical band gap energy.47
(αhν)n = A(hν − Eg) | (2) |
ERHE = EAg/AgCl + E0Ag/AgCl + 0.059 pH | (3) |
The overall photoelectrode efficiencies (ηoverall) representing the total yield of current generated in relation to the maximum current permitted by the absorption properties of the photoanodes were calculated from eqn (4), where Jph is the photocurrent at water oxidation potential (1.23 V vs. RHE) and Jabs was calculated from eqn (1).
ηoverall (%) = (Jph/Jabs) × 100 | (4) |
Fig. 1a–d shows the cross-section images of the pristine hematite (H), Ga-doped (Ga0.5H), Hf-doped (HHf3.0) and Ga–Hf-co-doped hematite (Ga0.5HHf3.0) thin films. The images show homogenous mesoporous morphologies for all samples, revealing commonly reported hematite worm-like nanograins.12,48 When comparing the films, it is apparent Hf4+ caused grain size reduction during the thin film production,49 a phenomenon commonly associated with ion segregation to interfaces.50 Ga3+ insertion does not cause crystal size reduction but promotes measurable increase in porosity. This suggests Ga3+ is predominantly doping hematite crystal lattice and could favor the active surface area for catalysis. The co-doped film showed a microstructure combining the individual effects of the dopants, for a relatively porous fine-grained structure.
Topological maps in Fig. 1e–h show the modification with Hf4+ reduced surface roughness in comparison to both undoped and Ga0.5H photoanodes (note the vertical z-direction scale bars). A similar result has been reported for Zr4+ in photoanodes produced by a polymeric precursor solution,12 with the smoother surface being attributed to better substrate wetting (smaller nanograins) and possibly correlated with more efficient electron collection at the back-contact. Current maps displayed in Fig. 1i–l highlight the synergistic effect of Ga3+ and Hf4+. While the single-doped hematite photoanodes showed limited electric conductivity enhancement, the Ga–Hf-co-doped photoanode exhibited uniform and constant conductivity pattern over the surface. This is likely an attribution of the spatial distribution of the dopants and their intrinsic electronic effects.
Fig. 2 shows the chemical composition mapping of Ga0.5HHf3.0_NiFeOx photoanode determined by energy dispersive X-ray spectroscopy (EDS) performed during scanning transmission electron microscopy (STEM) image acquisitions. The representative spectrum region where the chemical composition was evaluated shows Sn from the substrate (light blue) does not significantly diffuse into the hematite layer despite the thermal treatment, implying that any performance indicator cannot be attributed to Sn doping.51 The image also displays the oxygen (green) distributed over FTO and α-Fe2O3, iron (red) from hematite, and electrodeposited nickel (pink) spread over the photoanode surface. Gallium (yellow) is homogeneously distributed in the hematite grains as an indication of crystal lattice doping. Hafnium, though, besides segregating at hematite grain boundaries, is also found at the substrate–hematite interface, which would likely improve electrical contact and prevent electron loss due to FTO exposition to the electrolyte.52
Atomic concentration maps from Fig. 2 show gallium concentration between 0.2 and 0.45 at%. The average atomic concentration profile of three regions was calculated and identified by dashed windows (1–3) represented by their respective numbered graphs. Besides the concentrations in good agreement with the precursor added, it is remarkable the absence of Ga3+ at the surface. Hafnium atomic concentration maps identified by dashed windows 4–6 show that the average maximum concentration of Hf4+ segregated at the interfaces was approximately 6 at%, while at the FTO/hematite interface the average maximum concentration was 2.5 at%. As observed, the heterogeneous distribution of Hf4+ due segregation at polycrystalline grain boundaries and accumulation at the surface delivered atomic concentration distribution tending to zero towards the bulk (see x-axis of graphs 4–6). These results are particularly interesting, considering the stoichiometric control stablished by the synthesis method and its selectivity to deliver bulk and interfacial doping.
Furthermore, the observed dopant distribution has a cause-effect relationship with the conductivity maps presented in Fig. 1. As Ga3+ is dissolved in the lattice substituting Fe3+, it causes local negative strain due to it is relatively smaller ionic radius. Moreover, gallium–oxygen bonds are expected to be more ionic because of the difference in electronegativity, causing minor changes in the local energy levels and affecting polaronic migration for an improved conductivity.33 Since Ga3+ is not observed at the grain boundary regions, those remain similar to undoped hematite, showing high resistivity and annihilating benefits from the lattice doping across the film. Consequently, the conductivity profile shown in Fig. 1j for Ga0.5H is still within the picoampère (pA) range and similar to that for undoped hematite. Conversely, the large ionic radius of Hf4+ combined with its valence state are responsible for its segregation to grain boundaries, where it is expected to satisfy broken chemical bonds and ionic coordination.53 This grain boundary ‘healing’ effect decreases charge trapping across the grains by reducing the number of charge recombination sites, enhancing electron transport as observed in Fig. 1k. The Hf4+ impact becomes prominent when the synergistic effects with Ga3+ in the lattice are combined (Fig. 1l).
More in-depth understanding of the role of the dopants on the properties of the photoanodes was obtained from structural characterizations. X-ray diffraction (XRD) confirmed the crystalline phase α-Fe2O3 diffraction pattern indexed to the JCPDS card No. 33-0664 (rhombohedral crystalline system, space group Rc),54,55 with no detectable second phases associated with Ga3+ or Hf4+ (Fig. S2†). The diffraction patterns also remark the slight preferential growth in the (110) direction, due to its vertical orientation to the substrate.56
X-ray photoelectron spectroscopy (XPS) identified gallium and hafnium and the respective oxidation states in the photoanodes (Fig. 3). The doublet spin–orbit component corresponding to Fe 2p3/2 (between 710.6 and 711.2 eV) and 2p1/2 (between 724.0 and 724.6 eV) with respective satellite peaks at approximately 719 and 733 eV are typical of α-Fe2O3.57 The Fe 2p3/2 energy ∼14 eV lower than Fe 2p1/2 is characteristic of Fe3+ state, corroborating XRD data and consistent with hematite polycrystalline phase. XPS analysis was not able to reliably detect gallium 2p3/2 and 2p1/2 (ref. 58) in the high-resolution spectra, corroborating Ga3+ species are distributed in the interior of hematite grains rather than on the surface. Binding energies for Hf 4f7/2 (16.5 eV) and Hf 4f5/2 (18.1 eV) are somewhat lower than found for HfO2 in the literature,59 consistent with the existence of HfOx species (suboxides) in the surface of the photoanodes.
Moreover, a shift to lower binding energies is observed for Fe 2p3/2 and Fe 2p1/2 peaks of Ga0.5H, indicating Ga3+ is interfering significantly on Fe3+ chemical environment, i.e., doping the crystal lattice. A minor shift for Fe 2p3/2 and Fe 2p1/2 peaks of HHf3.0 can be attributed to the mentioned presence of hafnium suboxides at the surface, as indicated by Hf 4f high-resolution spectra. Hafnium atoms must dispute oxygen atoms in the surface for charge balancing, as the thermal treatment in inert atmosphere (750 °C, N2) for surface photoelectrochemical activation produces superficial oxygen vacancies, possibly distorting Fe–O bonds locally and slightly interfering in Fe3+ chemical environment.60 This result reinforces that hafnium is most likely to form excess at the interfaces rather than doping.
The Ga–Hf-co-doped photoanode has binding energies for the Hf4f peaks similar to the single-modified Hf sample, consistent with the hypothesis of non-stoichiometric hafnium oxides here as well (Fig. S3†). Moreover, the addition of both modifiers did not shift Ga 2p3/2 and Ga 2p1/2 or Hf 4f7/2 and Hf 4f5/2 binding energies when compared to single-modified photoanodes. This result supports the synthesis process can drive both modifiers to their specific role without creating conflicting drawbacks.
The designed dopant distribution was expected to affect the efficiency of the photoanodes. Interestingly, the absorption properties were not significantly affected by the modifications, as observed in the absorption profiles (Fig. S4†) and estimated optical band gap values (Fig. S5 and Table S1†). However, Fig. 4 shows the current density profile curves and photocurrent measured at 1.23 V vs. RHE (Jph) with clear improvements for the chemically modified photoanodes with optimized Ga3+ and Hf4+ content (see Fig. S6† for Ga3+ and Hf4+ optimization).
The photocurrent curves (Fig. 4a) show Ga3+ doping promotes a cathodic shift in the water oxidation onset potential of the photoanodes (∼100 mV), but the synergistic effect of Ga3+ and Hf4+ exhibit approximately the same onset as pristine hematite. This indicates Hf4+ features predominate over Ga3+ at the surface because it does not change the overpotential necessary for water oxidation. On the other hand, Ga3+ and Hf4+ addition considerably improved the photocurrent density throughout the water oxidation potential range (from 0.37 mA cm−2 for pristine hematite to 1.82 mA cm−2 for Ga0.5HHf3.0 at 1.23 V vs. RHE), indicating better electron injection to the external circuit. NiFeOx (photo)electrodeposition can enable the collection of minority charge carriers at lower potentials, and the passivation of surface-trapping states created by the addition of modifiers. It is apparent that NiFeOx improved the overall J–V curve by showing a shift in the onset to a lower potential and increasing the photocurrent response, suggesting that passivation of surface states occur prior to charge transport and transfer enhancement in the photoanode.61–64
The synergistic effect of the chemical modifications led to a photocurrent improvement up to 2.30 mA cm−2. While this number is still relatively modest when contrasted with the literature,4,5,65–73 the film thickness is only 176 nm, as shown in Fig. 1, representing a mass of material of less than 1 mg. This is a consequence of the high efficiency achieved by Ga–Hf-co-doping as illustrated in Fig. 4b by the overall photoelectrode efficiency (ηoverall). The overall photoelectrode efficiency values calculated from the ratio between Jph and the current values from light absorption (Jabs) does not correspond to the overall water splitting efficiency, since only the anodic photocurrent associated with the water oxidation processes taking place on the photoanode is considered. However, these values are extremely useful for comparing the total yield of current generated in relation to the maximum current permitted by the absorption properties of the photoanodes studied. In this work, for instance, while an incremental increase is provided when each dopant is individually introduced, the photoanode containing both Ga3+ and Hf4+ added by the polymeric precursor solution method showed 48% of overall photoelectrode efficiency, with NiFeOx bringing it up to 65%.
Fig. 4c and d show the overall photoelectrode efficiency of the optimized Ga0.5HHf3.0_NiFeOx photoanode compared to state-of-the-art hematite-based materials from the literature (Table S2†). Despite its modest photocurrent at 1.23 V vs. RHE and lower current generated due to light absorption (Jabs), the ηoverall of Ga0.5HHf3.0_NiFeOx is only rivaled by E-Ti-Fe2O3 photoanode,66 which was prepared by a multi-step process including hydrothermal synthesis followed by electrodeposition of CoPi and a subsequent KOH treatment. When compared with recent dual modification strategies reported in the literature (Table S3†),15,22,24,25,27–30,74–76 it becomes clear the new method leads to synergistic roles for Ga3+ and Hf4+, resulting in superior overall photoelectrode efficiency, as shown in Fig. 4e and f.
The Ga0.5HHf3.0_NiFeOx photoanode optimized by the selective doping was further tested to assess performance and structural stability over time using chopped illumination measurements (Fig. 5a) and operation tests for 3 h under illumination (Fig. 5b). Its reproducibility was also validated (Fig. S7†). Fig. 5c displays the amount of gas produced by this photoanode during 5 h operation, detected by gas chromatography.
As observed in the chopped illumination curves (Fig. 5a) and the chrono-amperometry measurements (Fig. 5b), the current generated by the engineered photoanodes is preserved in strongly alkaline media. These results validate the doping method in terms of incorporating modifications without damaging hematite well-known stability.12,64Fig. 5c further demonstrates the optimized photoanode can produce H2 and O2 with high faradaic efficiency, indicating almost all charge photogenerated is used for overall water splitting reaction. These results suggest structural and chemical stability of the photoanodes. To test this, the Ga–Hf-co-doped photoanode performance and surface composition were characterized before and after 3 h operation in the photoelectrochemical cell. Voltammetry measurement after stability test (Fig. 5d) corroborated the sustained performance indicated by the chrono amperometry, revealing identical photocurrent value at 1.23 V vs. RHE and same current density profile.
High resolution XPS spectra of Ga3+, Hf4+ and Ni2+ after the stability test (Fig. 5e–g) show that the surface composition remains unaltered during the 3 h of PEC operation. This result is summarized in Table 1. It is important to note that Ga3+ and Ni2+ percentages lie in the limit of detection of the XPS equipment, therefore determining their quantities is not trivial and the results in the table must be analyzed only for figure of merit and relative comparison. The presence of nickel was monitored only in the component Ni 2p3/2 because the doublet Ni 2p1/2 is not distinguishable from signal noise. The only measurable effect after the 3 h operation was a slight increase in –OH species adsorbed on the surface of the photoanode (Fig. S8 and Table S4†), as shown in the assigned peak centered at 532.7 eV,77,78 but no significant impact on the overall photoelectrochemical performance was observed. It is also interesting to note that the atomic percentages of Ga3+ and Hf4+ obtained by XPS analysis are in good agreement with the EDS average percentages shown in Fig. 2.
Sample | O (%) | Fe (%) | Gaa (%) | Hf (%) | Nia (%) |
---|---|---|---|---|---|
a Gallium and nickel percentages lie in the limit of detection of the equipment, therefore are not reliably detected. | |||||
Ga0.5HHf3.0_NiFeOx before 3 h operation | 68.16 ± 0.30 | 27.59 ± 0.30 | 0.16 ± 0.10 | 3.96 ± 0.10 | 0.13 ± 0.10 |
Ga0.5HHf3.0_NiFeOx after 3 h operation | 67.64 ± 0.30 | 28.06 ± 0.30 | 0.17 ± 0.10 | 4.02 ± 0.10 | 0.11 ± 0.10 |
Complementarily, a mechanistical overview on the role of the dopants was investigated by intensity modulated photocurrent spectroscopy (IMPS) performed under 30 mW cm−2 monochromatic illumination of a blue LED (λ = 470 nm). From the obtained data (see IMPS plot of pristine hematite in Fig. S10†), important parameters such as charge separation and transfer efficiency values were calculated using the IMPS general theory,79 accordingly described in Fig. S9† and presented in Fig. 6. As displayed in Ga0.5H photocurrent density profile (Fig. 6a), the onset potential cathodic shift when compared to pristine hematite is a signature of the reduction of polaronic effects, indicating the local symmetry break favored the electron mobility. Hence, charge separation (Fig. 6g) and transfer (Fig. 6j) efficiencies are mildly improved with a constant profile throughout the potential range of IMPS analysis, suggesting the local chemistry environment changes caused by Ga3+ addition can improve only the bulk conductivity. Analyzing the effect of Hf4+ addition, observed in both onset potential anodic shift in the HHf3.0 photocurrent density profile (Fig. 6b) and in the shift of charge transfer efficiency (ηtransf.) toward more positive potentials (Fig. 6k), there are indicatives that one of hafnium major roles is to form excess at the surface, thus creating surface states. Charge separation efficiency (CSExLHE) values for HHf3.0 (Fig. 6h) also confirm the other major role of Hf4+ which is its segregation at the hematite grain/grain interfaces. The reduction of the energy barrier heights at the grain boundaries introduced effectively enhanced electronic conduction and, therefore, charge separation efficiency.
From external quantum efficiency (EQE) values obtained under 30 mW cm−2 illumination at 470 nm for Ga0.5H (Fig. 6m) and HHf3.0 (Fig. 6n), it is evident the greater efficacy of segregation to overcome interfacial drawbacks over bulk doping since the electronic conduction is mainly limited by high energy barriers at the grain boundaries. Furthermore, the synergistic combination of both dopants resulted in a highly efficient photoanode with enhanced charge separation efficiency (Fig. 6i) and improved charge transfer efficiency (Fig. 6l).
The band edge positions (valence band maximum and work function) of the photoanodes (Fig. 7) were determined from ultraviolet photoelectron spectroscopy (UPS) spectra (Fig. S10†) with the input of bandgap energies (Eg) from Tauc plots. Gallium doping did not significantly displace the band edge positions but shifted the Fermi energy (EF) towards the conduction band (CB), justifying the increase in charge separation efficiency observed by IMPS analysis.32 This result is consistent with the assumption that gallium doping is reducing structural polaronic effects since small polarons are mainly responsible for hematite Fermi level pinning. For hafnium doping, there is an observable shift of valence band edge to a more negative value (VB = −7.34 eV) compared to pristine hematite (VB = −6.9 eV), which explains its superior PEC performance. On the other hand, the energy difference between the conduction band (CB) and the water reduction potential (−4.5 eV in Evacuum) for HHf3.0, which is 0.74 eV compared to 0.3 eV of pristine hematite, shows its requirement of a higher overpotential to drive the water oxidation reaction, corroborating the charge transfer efficiency profiles observed in Fig. 6k. Contrasting these findings with the profiles of J–V curves, it is possible to conclude the entangled relation between the band positioning of the semiconducting absorber materials and their photoelectrochemical behavior.
Fig. 7 Band diagrams obtained from UPS spectra of pristine hematite, Ga0.5H, HHf3.0, and Ga0.5HHf3.0. Valence band maximum and work function were extracted from the expansion of the region near the Fermi level and the determination of the secondary electron cutoff (Fig. S10†). Gap energies were extracted from Tauc plots. |
While the results are encouraging in this particular field, the nature of the proposed new polymeric precursor solution method possibly offers a powerful and overreaching synthetic alternative for the design of nanostructured materials with dopants purposefully positioned in strategic regions. This refined dopant addition could enable the simultaneous control of multiple challenges found in the nanostructures applied for device implementation, including improvement of electric contacts, increase in surface area and stability, manipulation of charge carrier densities, sintering of grains and passivation of surface states.
Footnote |
† Electronic supplementary information (ESI) available: Synthesis procedure; structural, optical, and photoelectrochemical characterizations; literature review; Tables S1–S4, and Fig. S1–S11† cited in the main text. See DOI: https://doi.org/10.1039/d3se00998j |
This journal is © The Royal Society of Chemistry 2023 |