aInstitute of Photonics and Nanotechnology, Vilnius University, Saulėtekio av. 3, LT-10257 Vilnius, Lithuania. E-mail: karolis.kazlauskas@ff.vu.lt
bInstitute of Chemistry, Faculty of Chemistry and Geosciences, Vilnius University, Naugarduko 24, LT-03225 Vilnius, Lithuania
First published on 22nd March 2022
Low-power NIR-to-vis upconversion (UC) of incoherent excitation mediated by triplet–triplet annihilation (TTA) has a variety of promising applications, e.g. in photovoltaics; however, these are strongly hampered by low UC efficiency in the solid state. The issue is mainly related to the most efficient rubrene annihilator (emitter) utilized for this spectral range, which experiences severe concentration quenching in films due to singlet fission (SF). Herein, a simplified thermal evaporation technique is introduced to alter the morphology of binary rubrene films without involving a singlet sink aiming to suppress SF and boost UC efficiency. Hot-plate evaporation of rubrene under ambient nitrogen on a Peltier-cooled substrate pre-coated with a sensitizer layer is demonstrated to significantly improve the FL quantum yield and triplet energy transfer after annealing, subsequently ramping UC quantum yield up to (1.2 ± 0.15)% (out of maximum 50%). This is at least twice as high as that found in any other binary NIR-UC film reported so far. Moreover, we find that the statistical probability (f factor) of producing a singlet from two triplets via TTA in amorphous rubrene films (f = 19.5%) is close to that estimated for rubrene in a solution. This finding infers a maximum UC yield of 1/2 × f ≈ 10% and explains why there are no reports on rubrene UC systems exceeding this value.
(1) |
Challenging practical TTA-UC applications, such as in photovoltaics, demand high NIR-to-vis UC efficiency, preferably in the solid state.8,26 A fulfilment of the latter requirement remains an important issue that many research groups aim to overcome. It is evident that the vast majority of demonstrated solid-state UC systems operating in the NIR range (>700 nm) usually express very low ϕUC, typically <1%.14,26–32
Commonly exploited TTA emitters for the NIR spectral range are tetracenes,33–35 rubrenes,24,30,31,36–40 perylenes26,41 or diketopyrrolopyrroles.42 Most of these emitters are efficient in the liquid environment. Meanwhile, there is a lack of emitters with a low lying triplet-state that are fluorescent in the solid state.14 The best-performing NIR-to-vis UC systems demonstrated so far, both in solution and the solid state, rely on the rubrene (Rub) emitter.14
Previously, we demonstrated that in the Rub-based UC solutions ϕUC is limited to ∼7.8% due to the relatively low f factor (∼15.6%).22 In the solid-state, however, Rub additionally suffers from severe concentration quenching mainly attributed to singlet fission (SF), which results in a more than 60-fold drop in the fluorescence quantum yield (ϕFL). Thus, even the most efficient Rub-based UC films typically demonstrate one or two orders of magnitude lower ϕUC compared to those of UC solutions, where ϕFL of Rub is almost unity.
Generally, SF related losses can be mitigated by using two approaches, i.e. (i) molecular engineering, which relies on the chemical modification of the existing emitters or the introduction of alternative ones; and (ii) physical engineering based on altering the UC film composition or morphology.
Previously, we utilized a molecular engineering approach to introduce t-butyl substituents into Rub and improve the NIR-to-vis ϕUC in the solid films.43 It was also revealed that Rub modifications at the periphery do not inhibit TTA step; however, substituents linked directly to the tetracene core suppress TTA dramatically.44 The standard physical engineering approach to combat low ϕFL in Rub films and mitigate SF is to introduce the third component, i.e. a singlet exciton sink (collector), dibenzotetraphenylperiflanthene (DBP). Doping Rub films with a low concentration of DBP was reported to boost ϕFL by a factor of 20 due to the efficient FRET of upconverted singlets from Rub to DBP.27,45 Yet, the potential for altering the UC film morphology by employing different preparation techniques to address low ϕUC issues was not exploited to the fullest extent.
In this work, we demonstrate the potential of the physical engineering approach to boost the UC efficiency in the binary emitter/sensitizer films without involving an exciton sink. To prepare UC films, we introduce a simplified thermal evaporation technique (using a hot plate) in an inert atmosphere. The highly concentrated Rub films obtained in this way display an order of magnitude higher fluorescence quantum yield (ϕFL) compared to the films produced by solution-processing or sophisticated thermal deposition in a vacuum. Furthermore, we show that in these films the sensitizer and emitter are well dispersed and intermixed to result in an efficient triplet energy transfer (ϕTET). The improved ϕFL along with the efficient ϕTET results in a record-high ϕUC of the Rub-based binary solid-state systems, which is at least twice as high as that obtained in any other binary NIR-UC film reported so far.14,32,46
It is well known that SF-associated losses are strongly related to the degree of crystallinity of the Rub films. The crystallinity can be altered by varying film preparation conditions and probed by monitoring their optical properties.
To minimize SF, amorphous Rub films with a chaotic molecular orientation and large average intermolecular distance must be produced. Biaggio et al. successfully exploited molecular beam deposition in a high vacuum to obtain amorphous Rub films.50 The films were virtually free from SF and showed mono-exponential fluorescence decay (τ = 16.4 ns) close to that of Rub in solution.50
In the current study, diverse deposition conditions of emitter Rub are investigated to assess the impact of emitter morphology on ϕFL, and correspondingly ϕUC in the solid films. Featuring an appropriate energy level alignment, palladium phthalocyanine (PdPc) was chosen as a triplet sensitizer for the Rub.43Fig. 2a and b illustrates the step-by-step fabrication of UC films under investigation. In the first step, the sensitizer layer composed of an optically inert polymer matrix doped with low concentration (0.1 wt%) of PdPc was formed by spin-coating (Fig. 2a). Then Rub was deposited on top by using one of the four distinct thermal evaporation modes to result in the formation of the UC film (Fig. 2b). In the vacuum deposition mode, controlled thermal evaporation in a high vacuum (∼10−7 Torr) was used. This mode was previously reported to produce amorphous rubrene films and therefore served as a reference deposition mode.50 The remaining three modes were based on a simplified thermal evaporation of Rub (using the hot-plate) in ambient nitrogen. In the cold deposition mode, rubrene molecules were deposited on a Peltier cooled (−10 °C) substrate (Fig. 2b). This mode is expected to instantly freeze emitter molecules on the substrate, thus producing amorphous films. Aiming to quantify the effect of substrate cooling, cold-deposited films were annealed at 100 °C defining the post-annealing mode. Lastly, Rub evaporation on an uncooled substrate (naturally heated due to the close proximity of the evaporation source) was named the hot deposition mode.
The UC films prepared at different conditions were initially evaluated by measuring FL transients and ϕFL (Fig. 3). The results clearly show high sensitivity to the Rub deposition mode. The FL transients consisted of the dominant prompt decay (fractional contribution of 70–90% to an overall decay) affected by SF and the minor slower decay component resembling natural decay of the isolated Rub species. The prompt component was described by a single-exponential decay profile to determine excited state lifetime. The shorter FL lifetime suggested an enhanced SF, and hence, a reduced ϕFL.
In the case of vacuum-deposited films, rapid decay with τ = 2 ns and low ϕFL (1.6%) was obtained. This was unexpected, since a vacuum-deposition previously was reported to result in amorphous films50 free from SF and with the FL lifetime similar to that of Rub in solution (τ = 16.4 ns).
Interestingly, prolonged decay (τ = 3.8 ns) as well as increased ϕFL up to 8.5% was obtained for the films fabricated using the cold deposition mode, indicating a more random molecular orientation and suppressed SF. Post-annealing of the UC films further extended the FL lifetime to 8.5 ns and improved ϕFL by almost 2-fold. Finally, the highest ϕFL of 20.5% along with the longest FL lifetime (τ = 12 ns) was determined for the films prepared in the hot deposition mode.
At first glance, the role of the heat treatment introduced during the film annealing or hot deposition is counterintuitive, since this is anticipated to facilitate Rub crystallization.51 Excess energy supplied in the form of heat may suffice to rearrange and crystallize Rub causing the formation of non-radiative SF centers. We note that the annealing temperature was set to correspond to the glass transition temperature (Tg) of the PS polymer employed. However, excess heat during the annealing can also promote Rub diffusion into the bottom sensitizer layer thereby diluting it and suppressing aggregation-caused FL quenching (see the inset of Fig. 4). Likewise, the hot deposition mode may result in a deeper Rub diffusion and thus stronger dilution more resembling the behavior of isolated Rub species or that of the purely amorphous film.
Further investigation in support of molecular diffusion involved studying the UC properties of the films via NIR excitation (730 nm) of the sensitizer. The improvement of UC efficiency was expected to be in correspondence with that of ϕFL. Indeed, the films of the lowest ϕFL fabricated using vacuum deposition and cold deposition modes exhibited barely detectable UC. On the other hand, annealed and hot-deposited films displayed bright UC. This result can be rationalized by considering the differences in the triplet energy transfer efficiency ϕTET (eqn (1)). The big temperature contrast during the cold deposition implies the formation of a bilayer UC film featuring a distinct boundary between the sensitizer and the emitter. As a result, most of the sensitizer triplets are generated far from the emitter species implying that short-range Dexter-type TET can only occur in a narrow interface region. Meanwhile, the promoted molecular diffusion during the film annealing causes mixing of the sensitizer and the emitter, thus reducing intermolecular separation and enhancing TET{PdPc → Rub}. Scanning electron microscopy (SEM) images supporting the mixing of the sensitizer and the emitter after annealing are provided in ESI† (see Fig. S1 and S2 and explanation therein). The mixing was also verified by evaluating ϕTET, where we compared phosphorescence intensity from the sensitizer PdPc of the cold deposited UC films with the same films after annealing (Fig. 4). For reference, we also measured phosphorescence of the emitter-free film containing only the sensitizer layer (polymer doped with PdPc). The experimental conditions ensured identical concentrations of PdPc and the sensitizer layer thickness of the tested films, thus enabling the intermixing effect of Rub and PdPc on TET to be addressed explicitly. The most intense PdPc phosphorescence peaked at 1106 nm was observed for the emitter-free film, since no TET{PdPc → Rub} was possible. Cold-deposited films expressed just a slightly reduced phosphorescence intensity due to inefficient ϕTET, whereas this intensity for the annealed films was severely decreased as a result of enhanced TET{PdPc → Rub}. Considering that
(2) |
Spatial variations of PdPc phosphorescence intensity and ϕTET in the annealed films are presented in the ESI† (see Fig. S4 and explanation therein). Taking into account the simplified thermal evaporation technique employed for the fabrication of the UC films, the reproducible ϕTET values could be obtained within the central area of ∼4 mm in size.
Even though the most efficient ϕFL was achieved using the hot deposition mode of Rub, the UC films prepared in this way had poor reproducibility. Specifically, Rub films were determined to be very sensitive to growth time and exhibited rapid crystallization already in the first growth stages (Fig. S5, ESI†). The morphological changes were accompanied by drastic spectral and FL decay time variations, i.e., additional aggregate-related FL band started emerging at 740 nm and τ reduced from 5.3 ns to 0.27 ns indicating increasing domination of SF.
Taking into account the reproducibility issues in the hot-deposition mode, further UC performance optimization was carried out for the films prepared by cold deposition followed by annealing. This deposition mode permitted control of the Rub thickness avoiding crystallization and allowed for consistent results (Fig. S6a, ESI†). Unlike neat Rub films obtained by the same method and showing increasing crystallization within a few weeks after fabrication, UC films fabricated by depositing Rub on top of the sensitizer-doped polymer layer followed by annealing were found to be stable. No signs of crystallization were detected several months after fabrication (see Fig. S7, ESI†) where FL lifetimes of the films are shown to remain constant at least within 240 days after film deposition). We attribute this to the dilution of Rub within the polymer layer, and thus suppression of rubrene aggregation.
Rub film thickness of approximately 600 nm, which corresponded to 3 min evaporation time was found to be optimal based on the UC intensity measurements (Fig. S6b, ESI†). Post-annealing of the films performed at 100 °C for ∼5 min yielded good film uniformity and bright UC emission, whereas longer annealing durations as well as higher temperatures induced strong crystallization (see Fig. S8, ESI†), and thus, were unacceptable for the UC film fabrication.
In the following UC optimization step, different sensitizer concentrations were tested while maintaining identical Rub deposition conditions (Fig. 5). Clearly, the increasing sensitizer concentration from 0.1 wt% to 5 wt% reduced the UC signal by 5 times suggesting enhanced upconverted energy back-transfer from Rub to PdPc. Although a higher sensitizer concentration is supposed to improve NIR absorption and reduce UC threshold, densely packed sensitizer molecules facilitate energy back-transfer diminishing the overall ϕUC.52 Aiming to maximize UC efficiency, the lowest PdPc concentration (0.1 wt%) was selected for further optimization. In fact, even lower concentration should potentially lead to a higher ϕUC; however, the subsequently decreased sensitizer absorption and thereby significantly weakened UC signal would compromise reliability of the results.
In the next step, the uniformity of the rubrene film deposited on top of PdPc-doped PS (sensitizer layer) was investigated. The measurements were carried out for different sensitizer layer thicknesses enabling the optimal one for maximal UC performance to be revealed. As discussed above, well mixed sensitizer and emitter films are required to have efficient ϕTET as well as high ϕFL of Rub. By assuming limited Rub diffusion into the sensitizer layer during the annealing, the too thick sensitizer layers could cause high absorption, yet likely reduced ϕUC due to lowered ϕTET. To verify this, we prepared a series of spin-coated sensitizer layers of different thickness, which was varied by altering mixture viscosity and spin coater speed. The film thickness was probed using AFM (see Fig. S9, ESI†). The Rub was deposited on top of the sensitizer layer through a circular metal spacer, forming a disk-shaped film (see the inset of Fig. 6). The prepared UC films were investigated by scanning across the surface in the x direction with the focused 730 nm laser beam and collecting the emission spectra as illustrated in Fig. 6.
The detailed scheme of this experiment is presented in Fig. S10 (ESI†). The measured spectra were analysed by discerning UC and FLPdPc spectral components peaking at 560 nm and 774 nm, respectively, and examining they relative intensities. Prior to FLPdPc analysis, the strong background signal due to the scattered excitation light and UC emission tail was subtracted.
The UC intensity was found to exhibit a steep increase by almost 3 orders of magnitude with the excitation spot moving from the film edge to the centre (Fig. 7a). The intensity profile resembled Gaussian-like thickness distribution of the evaporated Rub and suggested that some critical thickness of the emitter is required to promote TTA in the Rub layer. Additionally, the sensitizer layer thickness of 110 nm was determined to be the optimal as giving rise to the highest UC intensity at these deposition conditions. Spatial distribution of FL intensity emanating from PdPc was found to be much more flat (Fig. 7b) in agreement with rather homogeneous sensitizer layers formed by spin-coating. These layers contained roughly the same amount of PdPc across the scanned area implying insignificant FL intensity variation vs the excitation coordinate. Taking into account that FLPdPc is not affected by the presence of Rub due to the energy level alignment, FLPdPc intensity should be proportional to the sensitizer layer thickness and PdPc concentration. Since the latter was fixed at 0.1 wt%, the thicker sensitizer layers (as more absorbing 730 nm radiation) resulted in the higher FLPdPc intensity. Importantly, considering that ϕFL of PdPc is constant across the film, this intensity can be used as an internal reference for the UC signal, thereby enabling the judgement of ϕUC from the UC and FLPdPc intensity ratio (Fig. 7c). For instance, although 25 nm and 500 nm-thick films showed similar UC intensity, the thicker films exhibited higher FLPdPc intensity correspondingly implying lower ϕUC. Unfortunately, the FLPdPc signal of 25 nm films was too weak to be measured; however, the data presented in Fig. 7c clearly suggest that thin sensitizer layers are more favorable for the realization of high ϕUC.
We note that the UC films with thin sensitizer layers (<100 nm) were difficult to measure as they were highly scattering and featured weak absorption, and hence, a relatively low UC intensity. These layers acted as a buffer for evaporated Rub and had a significant influence on the final UC film morphology. During the Rub deposition thin buffer experienced partial melting thereby forming a rough surface with enhanced scattering of the incident radiation. Taking this into account, a sensitizer layer thickness of 110 nm delivering one of the highest UC/FLPdPc ratios was selected to be optimal for UC films. Measurement of UC intensity vs excitation power density for these UC films enabled to determine the UC threshold of 1.4 W cm−2 (Fig. S11, ESI†), which was found to be similar to those of other rubrene-based solid-state UC systems.27,28,43,46 The optimized UC films were subjected to further evaluation of ϕUC by using the FLPdPc signal as an internal quantum yield reference (Fig. 8) as well as by means of an integrating sphere. The methodological details for the determination of ϕUC using an internal reference are provided in the ESI.†
Fig. 8 illustrates the UC spectrum of the optimized UC film containing a 110 nm-thick sensitizer layer. Additional spectra of UC films with varying sensitizer layer thickness, prepared under otherwise the same conditions, are also shown for comparison. The UC spectra were normalized to the FLPdPc peak intensity so that UC intensity would correspond to ϕUC, as discussed earlier. Based on the independent measurements of UC films with different sensitizer layer thicknesses, yet with a fixed PdPc concentration of 0.1 wt%, the FL quantum yield of PdPc was determined (ϕPdPcFL = 0.1%). The reproducibility data of ϕPdPcFL tested for different films are included in the ESI.† Essentially, the data confirmed the average ϕPdPcFL to be 0.1% with a standard deviation of 0.03%.
Using this value as an internal reference, we could roughly deduce ϕUC to increase from 0.4% to 1% with decreasing sensitizer layer thickness from 500 to 110 nm (Fig. 8). The obtained ϕUC were confirmed by the measurements in the integrating sphere, where the most efficient UC film exhibited ϕUC = (1.2 ± 0.15)% (out of maximum 50%).
A slight underestimation of ϕUC by using an internal reference method can be explained by the strong background signal in the spectral region of FLPdPc due to the intense long-wavelength tail of UC emission. The accurate subtraction of such a strong background is complicated, which results in artificially increased FLPdPc intensity, and subsequently, somewhat reduced ϕUC. The calculated relative error for ϕUC in the case of the internal reference method was 32% (see the ESI†) implying that ϕUC values obtained by both methods agree well within these errors.
ϕ UC of (1.2 ± 0.15)% attained in this work represents a 17-fold improvement over our previous spin-coated DBP-doped rubrene films43 and at least a 2-fold improvement in respect to the most efficient binary rubrene-based solid-state systems reported to date (ϕUC ≈ 0.3–0.5%).14,29,46
We also note that the obtained ϕUC of the binary film approaches the highest efficiency value (ϕUC = 2%) achieved for the ternary UC film, additionally containing the DBP exciton sink.46 This reduces the gap in the performance of binary and ternary systems, minimizing the demand for the third component (singlet exciton sink) and stressing the importance of the UC film morphology rather than energetics of individual molecules.
Inserting the maximum efficiency values of the energy transfer/conversion processes determined for our UC films in eqn (1), the probability factor f for rubrene in the solid state can be estimated. Thus, taking into consideration that ϕFL = 20.5% (Fig. 3), ϕTET = 60% (Fig. 4), and ϕISC = 100% for palladium phthalocyanine-based sensitizers,22,39,41ϕTTA ≈ 100% in the TTA domination regime and that the maximal ϕUC = 1.2%, the statistical probability f to generate a singlet from two triplets via TTA is 19.5%. The confirmation for the deactivation occurring totally through the second-order path (ϕTTA ≈ 100%) achieved under excitation density of 100 W cm−2, i.e., well exceeding UC threshold is provided in the ESI.†
Interestingly, the obtained f factor is close to that estimated for rubrene in a solution (15.5%).22 This can be justified by the similar energy level alignment of rubrene in the different environment (solution or amorphous-like film) supporting the finding that the statistical probability of creating a singlet from two triplets via TTA should be in the range of 15–20%. We note that f estimated by us in the TTA-dominating conditions under continuous-wave excitation is 3–4 times lower as compared to that obtained under femtosecond pulsed-laser excitation conditions.38 The obtained f value implies a maximum ϕUC of 1/2 × f ≈ 10% for rubrene UC systems, which is reasonable, since no higher ϕUC has been demonstrated so far.14,27–32,46,53
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1tc05332a |