Qing
Wu
ab,
Karolina
Soppa
c,
Elisabeth
Müller
d,
Julian
Müller
e,
Michal
Odstrcil
df,
Esther Hsiao Rho
Tsai
dg,
Andreas
Späth
hi,
Mirko
Holler
d,
Manuel
Guizar-Sicairos
d,
Benjamin
Butz
e,
Rainer H.
Fink
h and
Benjamin
Watts
*d
aUniversity of Zurich (UZH), Rämistrasse 73, 8006 Zurich, Switzerland
bTH Köln – University of Applied Sciences, Ubierring 40, 50678 Köln, Germany. E-mail: qingaling@gmail.com
cBern University of Applied Sciences (BUAS), Fellerstrasse 11, 3027 Bern, Switzerland. E-mail: karolina.soppa@hkb.bfh.ch
dPaul Scherrer Institute (PSI), Forschungsstrasse 111, 5232 Villigen-PSI, Switzerland. E-mail: elisabeth.mueller@psi.ch; michal.odstrcil@psi.ch; mirko.holler@psi.ch; manuel.guizar-sicairos@psi.ch; benjamin.watts@psi.ch
eMicro- and Nanoanalytics Group, Universität Siegen, Paul-Bonatz-Strasse 9-11, 57076 Siegen, Germany. E-mail: julian.mueller@uni-siegen.de; benjamin.butz@uni-siegen.de
fCarl Zeiss SMT, Carl-Zeiss-Straße 22, 73447 Oberkochen, Germany
gBrookhaven National Laboratory, Upton, New York 11973, U.S.A. E-mail: etsai@bnl.gov
hFriedrich-Alexander-Universität Erlangen-Nürnberg (FAU), Egerlandstraße 3, 91058 Erlangen, Germany. E-mail: andreas.spaeth@fau.de; rainer.fink@fau.de
iInstitut für Nanotechnologie und korrelative Mikroskopie (INAM), Äußere Nürnberger Strasse 62, 91301 Forchheim, Germany
First published on 10th October 2022
Many European sculptures and altarpieces from the Middle Ages were decorated with Zwischgold, a bilayer metal leaf with an ultra-thin gold face backed by silver. Zwischgold corrodes quickly when exposed to air, causing the surface of the artefact to darken and lose gloss. The conservation of such Zwischgold applied artefacts has been an obstinate problem. We have acquired quantitative, 3D nanoscale images of Zwischgold samples from 15th century artefacts and modern materials using ptychographic X-ray computed tomography (PXCT), a recently developed coherent diffractive imaging technique, to investigate the leaf structure and chemical state of Zwischgold. The measurements clearly demonstrate decreasing density (increasing porosity) of the leaf materials and their corrosion products, as well as delamination of the leaves from their substrate. Each of these effects speak to typically observed issues in the conservation of such Zwischgold applied artefacts. Further, a rare variant of Zwischgold that contains extremely thin multiple gold layers and an overlapping phenomenon of Zwischgold with other metal leaves are observed through PXCT. As supportive data, scanning electron microscopy (SEM) and scanning transmission electron microscopy (STEM) coupled with energy dispersive X-ray analysis (EDX) were performed on the medieval samples.
A further innovation appeared in medieval Europe, whereby the gold leaf was backed by a relatively thicker, cheaper metal (usually silver) so that the expensive gold layer could be made thinner than contemporary gold leaf and hence reduced the gilding costs by at least half.2,3 This new laminated metal leaf has been known by many names in different languages, e.g. part-gold in English,4or parti in French,5,6 and oro di metá in Itatian,7 but is now commonly referred to by the German word Zwischgold.8–11 The production of Zwischgold is recorded to involve adhering a thin gold layer over a thicker silver base with a so-called “cold welding” technique.8,9 The materials for producing Zwischgold were supposed to be fine gold and fine silver12 and it is assumed that the gold was sourced from high quality gold coins, e.g. florins and ducats, in the same manner as contemporary gold leaf.13 The silver component makes Zwischgold susceptible to corrosion and its surface tends to darken and lose its gloss when exposed to air. This occurs because Ag atoms readily diffuse through the grain boundaries of the gold layer to reach the upper surface and then react with S and Cl in the presence of moisture.14,15 In regions where the local guilds did not prohibit the use of Zwischgold, the application of a protective varnish was usually a requirement.4,16 Since uncorroded Zwischgold applications are difficult to distinguish from gold leaf, it is probable that many Zwischgold examples remain unrecognised. However, many of the known late medieval Zwischgold-applied artefacts present a matte black surface, likely due to the degradation of the organic varnish materials over the centuries and subsequent silver corrosion.
The application of Zwischgold in artworks began on paintings of the early 13th century4 and became popular in German sculptures from the 14th century.17 Since it presents a real gold surface while requiring much less gold than normal gold leaf, it is typically thought that it was mainly used at the time as an economical alternative to gold leaf.4,8,18–20 This theory is supported by many examples of Zwischgold being applied to less prominent areas, such as the rear or within concave clothing folds of altar sculptures,21–23 especially with its corroded, darkened appearance that can be easily distinguished from the surrounding gold leaf surface. However, modern scientific analysis reveals that Zwischgold has also been applied prominently, for example, in the Leiggern Altar from the Swiss National Museum (SNM) presented in Fig. 1a, the entire outer gown of the central Mary figure, the clothes of three floating angels, hair/beard of some wing figures, and the top frames of the shrine were applied with Zwischgold.24–26 In such a case, economic considerations seem less convincing. The complexity of Zwischgold's structure and the reasons for its application make it an interesting topic for research in art history and art technology.
The techniques for applying Zwischgold onto its substrate were similar to those for gold leaf, among which the bole gilding and oil gilding techniques were most commonly used.4,27 Bole gilded Zwischgold leaves were directly applied on the bole substrate with an aqueous solution and, once dry, burnished with agate or animal horn to smoothen the surface to a high gloss. Fig. 1b presents typical examples of Zwischgold applied to limited areas of two late medieval gilded sculptures, showing dark patches where silver has diffused through to the surface and strongly tarnished.15 One of the very few exceptions is the central figure Mary of the Leiggern Altar, which still appears golden in colour (if somewhat dark) and retains gloss. As such, Mary provides a good opportunity to obtain a sample that is well known to contain medieval Zwischgold that has not been heavily corroded.
Ptychographic X-ray computed tomography (PXCT) is a 3D imaging technique that, instead of using image-forming optics, uses iterative mathematical routines to analyse the X-ray scattering patterns of a sample as a function of rotation and translation to reconstruct a full 3D image of the refractive index variations within the sample.28–31 The resolution of ptychography is not given by the scanning step nor by the beam size, as with scanning probe microscopy, but rather by the widest-angle scattering observed that correspond to the shortest-length features, or sample variations.32,33 PXCT is thus among the X-ray techniques with the highest resolving power.34–37 PXCT provides a quantitative measure of the complex-valued refractive index (both absorption β and refraction δ) distribution in a specimen. Measurements performed with hard X-rays tend to show higher contrast in δ due to the high penetration power (low absorption) of hard X-rays. While measurements using an X-ray energy close to an elemental resonance can be used to increase sensitivity to particular materials, utilising an X-ray energy far from such resonances will provide β and δ values that both correlate roughly proportional to the mass density of the sample materials. Hence, given some foreknowledge of the sample composition, the identity of a material can be inferred from the measured local δ values, together with variations in composition and/or porosity.30
Due to its ultra-thin leaf thickness (e.g., 500–700 nm for modern Zwischgold15 and significantly thinner for medieval Zwischgold38), a characterisation of Zwischgold requires both high resolving power and high sensitivity and is thus challenging for conventional techniques. Recent work by our collaboration group15,26,38,39 has demonstrated the use of modern analytical techniques such as SEM-EDX to identify and characterise modern and historical Zwischgold including its leaf structures and layer/leaf thicknesses, as well as its complicated individual ageing phenomena. These typically involve the formation of silver compounds that can be distributed evenly or in aggregates in regions surrounding the gold layer, and consumption of the silver base which leads to delamination of the metal leaf from the substrate. However, the 2D cross-sectioning techniques provide only a limited view of the whole, complex scenarios that are observed in historical Zwischgold samples. Three dimensional imaging will certainly provide more informative views of real objects than 2D cross-sections, although the degree to which this is useful has not yet been fully explored since nanoscale 3D imaging is relatively new and still not easily accessible. Further, sectioning historical Zwischgold samples is challenging due to the fragile nature of the specimens; the substrates can be porous and brittle and the leaf poorly adhered, while the corrosion products and organic overlayers can be chemically and mechanically unstable. Hence there is a strong possibility for any sectioning technique to alter the sample materials and structures at the cutting face. Therefore, we have applied PXCT to both modern and historical Zwischgold samples, so that the structures and chemical states of the Zwischgold and surrounding materials can be observed in quantitative, 3D nanoscale images. The PXCT will provide valuable observations of interior regions of Zwischgold samples away from the cutting face and thus test the validity of previous Zwischgold observations by conventional techniques. The quantitative nature of the PXCT data will also provide opportunities for novel observations.
Two freestanding Zwischgold leaves (Recent and 10-year) were included in the modern samples: one recently manufactured (using 23.2 carat gold; Noris Blattgold, Germany), and another manufactured approximately 10 years ago (manufacturer unknown). Both of these had been stored in their original packaging in a cool, dry cupboard. A third modern sample (35-year) was taken from an unvarnished and strongly corroded area of a 35-year old Zwischgold demonstration object at the Bern University of the Arts. The Recent and 35-year old Zwischgold samples have been characterised in a previous publication.15 Although the original manufactured purity of the Au layer in the 10-year and 35-year old Zwischgold samples are not precisely known, it is very likely that the tradition of using high-purity gold and silver was followed and they are similar to that of the Recent Zwischgold sample. Elemental analysis by Energy Dispersive X-ray (EDX) and X-ray Fluorescence (XRF) analysis (see Fig. S1 and S2 in the ESI†) did not reveal significant amounts of other metals, especially copper, which would be the most likely indicator of lower-quality gold and silver.40,41
The Leiggern Altar (Fig. 1a) is thought to have been produced in the region of Ulm, Southern Germany in 1420.42 At the time of its purchase by the Swiss National Museum in 1925, it was displayed in the Leiggern mountain chapel in Ausserberg (Valais, Switzerland) and from 2019 has been on permanent exhibition in Zurich. The altar figure Mary (size: H 112.5 × B 44.5 × D 25 cm) stands at the centre of the Leiggern Altar. Previous X-ray fluorescence measurements indicated extensive use of gold, silver and Zwischgold leaves.25 The Zwischgold-applied outer gown of Mary appears well preserved, but is known to have been partly applied with gold leaf during restoration treatments in the past; hence the sample Mary was taken from an area, indicated in Fig. 1a by a green arrow, where we expect that only original Zwischgold is present.25 A 1974 investigation24 on the altar figure Mary described an organic varnish layer applied to the top surface of the object, which has been confirmed by our SEM-EDX measurements showing significant amounts of C and O in the top layer of a sample cross-section (see Fig. S5 in the ESI†). SEM measurements further provide evidence for a presence of Fe-containing particles in the substrate and Zn-containing particles in the varnish (see Fig. S5†). The former indicates the use of bole gilding techniques.8,43,44 The source of Zn-containing particles is uncertain; possibly some Zn compounds were used as siccative during the drying process of an oil-based varnish.45,46
Two 15-century polychrome wooden sculptures St. Bishop and St. Nicolaus were acquired by the Historical Museum Basel (HMB, Switzerland) via a private donation from Sedrun (Grisons, Switzerland) in 1941.47 Further details of their origin and history are not available. Fig. 1b shows that these sculptures contain dark, matte patches on their golden gowns, which is indicative of corroded Zwischgold. Two samples (Bishop and Nicolaus) were taken from the centre of a darkened patch on each object and an extra sample (Nicolaus Border) was taken from the border area of a darkened patch next to the neighbouring gold surface. These three samples exhibit much stronger corrosion phenomenon than the Mary sample, which can be easily discerned by eye and has been further confirmed through the SEM-EDX measurements (Fig. S12, S13 and S14 in the ESI†).
Fig. 2 (a) Segmented PXCT 3D view and (b) depth profile of the Recent sample. (c) Segmented PXCT 3D view and (d) stack plot of the depth profile of the 10-year sample. (See Fig. 3 for further segmentation details.). |
Further detail can be seen in Fig. 3, which presents δ histograms from PXCT measurements of the gold reference together with the Recent, 10-year and 35-year modern Zwischgold leaves. The main materials of interest, namely the metallic Au and Ag, are expected to be observable in peaks located at δ-values of approximately 40 × 10−6 and 25 × 10−6, while the main corrosion products (i.e., Ag2S and AgCl) are expected to be significantly porous and so should produce peaks at δ-values lower than the 17.6 × 10−6 and 13.6 × 10−6 calculated from their respective bulk densities. Previous EDX measurements15 and complementary XPS measurements (see Fig. S16†) confirmed the dominance of Ag2S in the 35-year sample and therefore the peak centred at 15 × 10−6 is attributed to Ag2S. Since this Ag2S peak position has a δ-value approximately 15% lower than expected for the bulk material, we conclude that the observed material has a 15% decrease in density due to porosity below the resolution of this measurement. The weak peaks observed near 10.5 × 10−6 in the 10-year and 35-year histograms would fit to AgCl with a similar porosity to that of the observed Ag2S. The peaks at δ-values of 7.0 × 10−6 and 7.9 × 10−6 in the 35-year histogram are attributed to materials in the substrate, while the peak near 5.7 × 10−6 is due to the carbon layer deposited on the sample surface to protect it from Ga+ ion implantation during sample preparation by focused ion beam (FIB) milling. Air surrounding the measured samples produces a strong peak at a δ-value of zero. Table S1 in the ESI† lists additional candidate component materials and their calculated X-ray refractive indices.
A striking trend in the histograms in Fig. 3 is that the right-most (highest δ) peak, which corresponds to the highest density material observed in the samples, only matches the δ-value calculated for bulk gold in the case of the pure gold reference sample. The Recent and 10-year leaf samples show their highest-δ peaks at 36.5 × 10−6 and 32 × 10−6, respectively, while the 35-year sample shows only a monotonic decline as the δ-value increases above the Ag peak position. While this is partly due to the smaller amount of gold present in the older samples, blurring and volume-mixing artefacts of the imaging technique tend to reduce the apparent δ-values of the Zwischgold gold layers, especially those that have a similar thickness to the imaging resolution (see Table 1) and are surrounded by much lower-δ materials. The alternative explanation that the gold is significantly decreasing in density or purity with time is contrary to the well-known chemical inertness and low diffusivity of gold lattices.48–51 Indeed, STEM-EDX measurements of the medieval Mary sample, discussed in detail in the following section, demonstrate that the gold layer of Zwischgold retains its purity and density over long time scales.
Sample | FOV (H × V μm) | Step size (μm) | Projections | Time (h) | Pixel size (nm) | 3D FSC (1/2 bit; nm) |
---|---|---|---|---|---|---|
Recent | 13 × 6 | 0.6 | 820 | 15 | 12.12 | 18 |
10-year | 13 × 6 | 0.7 | 870 | 18 | 20.27 | 24 |
35-year | 15 × 6 | 0.6 | 700 | 13.2 | 15.3 | 35 |
Mary | 10 × 5 | 0.6 | 480 | 6 | 15.3 | 30 |
Bishop | 12 × 6 | 0.6 | 400 | 6.8 | 15.3 | 39 |
Nicolaus | 10 × 5 | 0.6 | 800 | 9.8 | 15.3 | 19 |
Nicolaus Border | 12 × 10 | 0.6 | 548 | 14.3 | 15.3 | 36 |
Au reference | 6 × 6 | 0.6 | 160 | 1.7 | 15.3 | — |
More subtle movement of the Ag peak is also observed in Fig. 3, shifting from 24.8 × 10−6 in the Recent sample, to 24.4 × 10−6 in the 10-year sample and to 24.5 × 10−6 in the 35-year sample, indicating a 1.6%, 3.2% and 2.8% respective decrease from the δ-value of 25.2 × 10−6 calculated for bulk Ag. This decrease is interpreted as an increase in porosity in the Ag, due to the Kirkendall effect.52 The Ag peak of the 35-year histogram is also much lower and broader than the Recent and 10-year ones; since the broadening is roughly symmetric and porosity can only make a material less dense (i.e. move a voxel to the left in the histogram), we expect that this is also an effect of the imaging resolution.
Fig. 4 displays segmented 3D visualisations from PXCT measurements of the 35-year Zwischgold sample, with exposed cross-sections and stepwise addition of materials in order to highlight details in each layer. These tomograms have been segmented according to the δ-ranges indicated by the colour bar along the bottom of Fig. 3. The view in Fig. 4a shows only the red “Au” segment, while the view in Fig. 4b adds the blue “Ag” segment and shows translucent surfaces of the internal voids (which are shown in orange in Fig. 4d). Fig. 4c displays the Au and Ag segments together with the green “silver sulphide” segment (centred on the 15% porous Ag2S peak). Finally, Fig. 4d displays all material segments, including the greyscale segments attributed to the bole, varnish and FIB-protection materials. Internal voids are shown as an orange segment. While the Recent and 10-year leaf samples (Fig. 2) display consistent and even layers of gold material over silver, the gold layer of the 35-year sample (Fig. 4a) is much thinner and shows strong thickness variations and no longer appears to form a continuous layer (or perhaps gets thinner than the imaging resolution). Fig. 4e shows an area-integrated depth profile (aligned to the upper surface of the gold layer) of the single-layered section of the 35-year sample that demonstrates the proportions of the material segments as a function of depth below the leaf surface. The FWHM thickness of the Au segment gives a gold layer thickness of 47.9 nm, which is similar to the 3D Fourier shell correlation estimate of the PXCT image resolution of 35 nm (see Table 1) and suggests that the observed FWHM gold layer thickness is not reliable. The observed gaps in the Au segment in Fig. 4a could also be a consequence of insufficient imaging resolution rather than actual gaps in the gold layer of the Zwischgold leaf. Fig. 4e shows a depth profile of a single-layer section of the 35-year sample; here we see a second red Au segment peak near 400 nm depth that indicates a thin layer of increased δ-value at the lower edge of the silver layer (also visible on the left edge of the leaf in Fig. 4b). One could speculate that this thin layer is gold material transferred to the bottom of the leaf by contact with gold-contaminated manufacturing equipment.
Fig. 4 PXCT 3D images of the 35-year old Zwischgold sample showing the addition of (a) Au, (b) Ag (with transparent voids), (c) “silver corrosion products”, and (d) other segments (see Fig. 3 for segmentation details). (e) Stack plot of the depth profile of the single-layered section of the sample, aligned to the main layer of the Au segment. |
Adding the Ag segment in Fig. 4b shows that a significant amount of the silver backing layer of the Zwischgold leaf remains intact. A flattened, S-shaped crease can also be observed in the metal leaf towards the right-hand edge of the tomogram. Wrinkles are commonly formed when a gilding leaf is initially laid onto the substrate and the surface is typically then burnished (rubbed with a tool) in order to flatten and compress these wrinkles to obtain a flatter, more shiny surface. The crease observed in Fig. 4 is approximately 2 microns wide at the front edge of the sample and gradually narrows to a point at the sample's rear. Burnishing of the surface also appears to have dragged some metal across the trough next to the creased leaf, demonstrating that burnishing a metal leaf surface can do more than simply compressing ridges. This burnished surface layer is also visible in distribution of Au and Ag in the depth profile between −250 nm and the surface of the main gold layer.
Adding further components to the tomogram in Fig. 4c and d, we observe a layer of silver sulphide (green) over the metal layers and a few clusters below. The dark grey clusters just below the metal leaf appear consistent with porous silver chloride in both δ-value and spatial arrangement. Previous measurements of corroded Zwischgold have shown that the silver sulphide layer becomes substoichiometric close to the metal interface.15 The δ-values used to segment the PXCT data scale roughly linearly with material density and so it is not possible to distinguish between small changes in elemental composition and variations in material porosity. Examining the orange segment representing internal voids in Fig. 4d, we clearly observe a significant gap that has opened between the metal leaf and the bole substrate. The extent of the gap can also be clearly seen in the depth profile, where the void occupies approximately 85% of the cross-sectional area just below the metal leaf. Previous observations of such gaps in neighbouring sections of the same sample15 showed a much smaller separation that was consistent with consumption of the silver layer, however, the gap observed here clearly involves mechanical movement of the metal leaf away from the substrate. We hypothesise that the gap observed here may have been caused, or increased, by differential expansion and contraction of the metal leaf and the substrate during temperature and humidity cycles over the lifetime of the object. While it is possible that heating of the sample during FIB preparation53 is at least partly responsible for the separation of the metal leaf from its bole substrate, similar measurements on the medieval Zwischgold samples did not show the same pattern of voids in all cases and so indicate that the observation of leaf-substrate separation is likely not just an experimental artefact.
Fig. 5 PXCT 3D images of the Mary sample showing the addition of (a) Au, (b) Ag (with transparent voids), (c) “silver corrosion products”, and (d) other segments (see Fig. 7 for segmentation details). (e) Stack plot of the depth profile of the sample, aligned to the main layer of the Au segment. |
Fig. 6 STEM-EDX analysis of a sample taken in an adjacent region to the Mary sample: (a and b) EDX elemental maps for Au and Ag, and EDX spectra of area 1 and 2; (c and d) EDX elemental maps for Au and Ag, and EDX spectra of area 3 and 4; (e–g) EDX Au and Ag maps and high-angle annular dark-field (HAADF) image of a gold grain boundary filled with silver atoms; (h) EDX line profile across a gold layer grain boundary (along the green arrow). Sub-panels (e–h) reproduced from ref. 38. |
Further evidence of the limits of the PXCT analysis is provided by an EDX analysis through STEM (operating with a resolution of a few nanometers) on a sample taken in an adjacent region of the Mary sample, shown in Fig. 6. Fig. 6a–f demonstrates that there is a clear separation between the gold and silver layers and that these layers have purities of more than 98 at% and 99 at% respectively. Such observations indicate that no significant lattice interdiffusion has occurred in this 600-year old Zwischgold sample. However, grain boundary diffusion is expected to occur rapidly and can be observed in Fig. 6e–h as a narrow line of Ag crossing the gold layer at the boundary between crystalline grains. The grain boundary is observed to be about 5 nm wide and so grain boundary broadening cannot be a significant contribution to the strong gold-thickness variations observed in the Mary sample.
The distribution of (green) silver sulphide in the Mary sample (Fig. 5c) shows two modes. The surfaces of the metal leaf are covered by a very thin layer of corrosion products, but there are also some bulk regions where the metallic silver layer of the leaf has been replaced by silver sulphide. The layers adjacent to the Zwischgold leaf in the Mary sample also show interesting features in Fig. 5. The supporting substrate is much more structured than that of the 35-year sample, showing higher δ-valued grains within a lower density matrix that contains a well-connected pore network with voids on the scale of 100–300 nm. Further, the depth profile in Fig. 5e demonstrates that these voids show a concentration at the underside of the metal leaf that reaches over 50% of the total leaf area, meaning that less than half of the leaf area remains attached to the bole substrate. The relatively low-δ and smooth varnish layer similarly shows pores and although they are also concentrated close to the leaf interface, they are much less connected and only sum up to 11.2% detachment of the leaf-varnish interface. These voids do not correlate with the consumption of the silver layer, and are more consistent with mechanical detachment via differential expansion-contraction as discussed above for the 35-year PXCT.
Examining the histograms of the medieval Zwischgold samples in Fig. 7, we observe a similar set of peaks to that of the modern samples, but with much lower counts at the δ positions corresponding to Ag and Au and an additional peak located at a δ value of about 10 × 10−6. While the Nicolaus Border shows a strong profile extending to very high δ values, the PXCT images in Fig. 8 reveal a completely different situation from the other samples where the main gold segment is below the silver segment and in some places separates into up to 3 layers. A clearer view of these layers is provided in Fig. 9 with a slice through the PXCT tomogram (a and b) and an SEM image (c) of a separate cross-section region of the Nicolaus Border sample, revealing that there are in fact three gold layers; the lowest layer is about 106 ± 24 nm thick, while the middle and upper layers are about 41 ± 16 nm thick. The mismatch between PXCT and SEM data in Fig. 9 clearly demonstrates that the high δ of these thin gold layers has been blurred across adjacent PXCT voxels, which effectively shifts the high-δ counts of the corresponding histogram in Fig. 7 to lower δ, where they fall into another segmentation bracket. Complementary EDX analysis of the Nicolaus Border sample (Fig. S12 in the ESI†) further reveals that a mixture containing elements Ag, S, Ca, O and C deposits mainly above the top gold layer. Such observations indicate that a two-layered Zwischgold leaf overlaps a normal gold leaf, and the metallic silver in the Zwischgold leaf has largely transformed into silver corrosion products (e.g. Ag2S), mixing with the varnish materials. This is consistent with the fact that the sample was taken from a border area between surfaces applied with Zwischgold and gold leaf. The presence of the gold leaf provides a significant number of gold voxels, contributing significantly to the highest δ segment of the histogram and exhibiting a similar profile as the Mary sample. The Mary histogram does not show a distinct peak for silver sulphide, but rather shows a gradual transition between the Ag peak and the δ-position of the 15% porous Ag2S peak observed for the 35-year sample, indicating significant variation in the stoichiometry and porosity.
Fig. 8 (a–d) PXCT 3D images for different components (see Fig. 7 for segmentation details) inside the Nicolaus Border sample. (e) Stack plot of the depth profile of the sample, aligned to the main gold layer. |
Although EDX analysis identifies silver sulphide as the main silver corrosion product in the Nicolaus Border sample, no peak is visible at 15 × 10−6 in the histogram presented in Fig. 7 as we have observed for 15% porous Ag2S in Mary sample. We do, however, see a peak at 12.1 × 10−6 that is spatially associated with regions close to the silver segment in Fig. 7 and so probably consists of Ag2S that is either twice as porous (31%) or is mixing with lower delta materials from the varnish. Our SEM-EDX observations indicate that each of these possibilities typically occur in different sites of each sample. SEM-EDX observations on different sites of this sample show that S is spread quite evenly throughout the entire varnish layer and so the peak at delta value 9 × 10−6 could perhaps also be described as corresponding to a mixture of Ag2S and organic varnish.
The Nicolaus sample taken from the centre of a corroded Zwischgold patch, Fig. 10, shows an extremely thin layer of high-δ voxels segmented into the Ag2S, Ag and Au segments. This is also reflected in the histogram presented in Fig. 7, where the histogram drops rapidly above a δ value of about 17 × 10−6 due to the very low proportion of high δ voxels. This thin layer is consistent with a single Zwischgold Au-layer matching the two Zwischgold Au-layers that overlay the gold leaf in the Nicolaus Border sample. However, complementary SEM-EDX measurements on a sample cross-section that was taken in an adjacent region of the Nicolaus sample, show that the Zwischgold leaf contains both single and double Au layers (Fig. S11a and b in the ESI†), and their average layer thickness of 29 ± 10 nm (Fig. S11c†) is consistent with the PXCT data. Previous SEM-EDX measurements of the Ag:Au elemental ratio provide an estimated original total leaf thickness of 225 ± 78 nm.38
Fig. 10 (a–d) PXCT 3D images for different components (see Fig. 7 for segmentation details) inside the Sedrun Nicolaus sample. (e) Stack plot of the depth profile of the sample, aligned to the metal layer. |
Unlike the 35-year and Mary samples, both of the Nicolaus samples display only a few, poorly connected pores in the varnish and bole layers. Further, these pores do not show significant concentration adjacent to the Zwischgold leaf in these two Nicolaus samples, demonstrating that the voids and delamination effects observed in other samples are not simply due to the sample preparation methods.
The PXCT data of the Bishop sample presented in Fig. 11 shows another highly corroded Zwischgold leaf that appears similar to the Nicolaus sample and has a thickness similar to the measurement resolution of 39 nm (see Table 1). Close inspection of the gold layer in a FIB cross-section of a Bishop sample by STEM reveals a triple-layer structure, as shown in Fig. 12, with an average thickness of about 16 nm for each gold layer. This fine structure is below the resolution of the PXCT measurements and suggests that the Zwischgold leaf applied to the Sedrun St. Bishop belongs to a rarely-observed class of multi-layered Zwischgold leaves.39 It is worth noting that the green segment representing corrosion products observed in Fig. 11 does not only reside above the original metal leaf position but is also distributed throughout the substrate, in the form of small aggregates. These aggregates distributed throughout the substrate could also be relatively large grains of iron oxide mixed with the bole substrate, since Fe2O3 has a δ value of 13.5 × 10−6. A few large-sized voids and lots of smaller pores are present around the metal leaf and throughout the substrate of the Bishop sample, though with less delamination of the leaf than was observed in the 35-year and Mary sample.
Fig. 11 (a–d) PXCT 3D images for different components (see Fig. 7 for segmentation details) inside the Sedrun Bishop sample. (e) Stack plot of the depth profile of the sample, aligned to the upper surface of the metal layer. |
The Mary sample, taken from the central figure of the Leiggern Altar is quite similar in thickness and structure to the modern Zwischgold, albeit with more lateral variation in the thickness of the gold layer. The Sedrun Nicolaus and Bishop samples, in contrast, are much thinner and are composed of multiple layers. Further study is required to determine if the Sedrun sculptures are of novel construction, or if ultra-thin, multi-layered Zwischgold leaves are actually more common than is currently understood. The thickness of the metal layers observed by PXCT was reasonably precise in cases where the measurement resolution was well below the layer thickness. However, one of the practical limits to the measurement resolution is the mechanical stability of the sample while measuring the set of projections, which was found to be unpredictable for historical samples. Complementary electron microscopy measurements proved invaluable for observing the fine, ultra-thin details of the historical Zwischgold leaves. Together, these observations provide insight into the relative value of higher resolution versus higher dimensional imaging techniques that can guide future studies.
The 3D imaging of PXCT also allowed us to assess the degree of adhesion (or connectedness) between the Zwischgold leaves and their bole substrates and varnish overlayers. Each of the samples that included a substrate displayed a series of voids within the substrate materials that were often concentrated near the leaf interface in a way that could be described as a partial delamination of the metal leaf. The 35-year and the Mary samples displayed 84.7% and 53.9% delamination area (respectively) at the leaf-substrate interface, while the Bishop sample presented a 45.5% fracture surface about 750 nm below the metal leaf. The delamination patterns appear more consistent with expansion-contraction tensions, rather than being connected to corrosion mechanisms. A concentration of voids near the leaf-varnish interface was also observed in the Mary, Nicolaus Border and Bishop samples, covering 11.2%, 5.3% and 5.5% of the respective interfacial area. The quantitative nature of the PXCT data further allowed estimation of the porosity of the corrosion products (e.g. 15% porous silver sulphide observed in the Mary sample) and even of the metallic silver (due to the Kirkendall effect).
This work has demonstrated PXCT as a powerful tool for quantitative three-dimensional characterisation of very heterogeneous samples. While the resolution of our measurements was not sufficient to fully resolve the very fine details of the Nicolaus and Bishop Zwischgold foils, there are a number of ways to improve future PXCT measurements. Firstly, cryo-preservation of the sample will help stop the sample from moving or changing shape during the measurement (this can happen due to radiation damage). Similarly, a more coherent X-ray source (from a diffraction limited synchrotron56) will improve the dose-efficiency of the PXCT measurements so that less radiation damage should occur. Secondly, improvements in the measurement rate due to improvements in detector hardware and photon flux of the X-ray beam can increase the rate of measurements so that further projections can be measured in the same amount of time. Finally, the reconstruction codes for analysing ptychographic and computed tomography datasets are undergoing rapid development that make them more tolerant of non-idealities in the raw data so that imaging artefacts can be minimised.
PXCT experiments35,58 were carried out at the cSAXS beamline (X12SA) at the Swiss Light Source, Paul Scherrer Institut (PSI), Switzerland. A general description of the PXCT measurements is given as follows. A double crystal Si(111) monochromator was used to provide a monochromatic radiation of 8.7 keV generated by an in-vacuum undulator. The beam was focused by a Fresnel zone plate (FZP) with a diameter of 120 μm, outermost zone width of 60 nm (ref. 59) resulting in a focal distance of 51 mm. The FZP was fabricated in the Laboratory for Micro and Nanotechnology, Paul Scherrer Institut, Switzerland. The sample was placed 1 mm downstream of the focus to give an illumination of approximately 2.5 μm in diameter. The ptychography scans followed a Fermat spiral pattern60 with an average step size of 0.6 μm over a field of view (FOV) of up to 15 μm horizontally by 6 μm vertically. Diffraction patterns were collected 7.4 m downstream of the sample using a Pilatus 2M detector61 with an exposure time of 0.1 s. Projections were measured at uniform intervals of sample rotation from 0° to 180°, with about 4 × 107 incident photons per square micron, per projection. The ptychographic reconstruction of the 2D projections from sets of 400 by 400 pixel diffraction patterns was performed using the difference map28 and maximum likelihood62,63 methods to give an image pixel size of 15 nm (except for the Recent and 10-year samples with voxel sizes of 12 and 20 nm respectively). Subsequently, projections were aligned64,65 to give 3D tomograms based on modified filtered back projection.64 The tomogram half-pitch resolution was estimated by Fourier shell correlation half bit criteria66 to be between 18 and 35 nm, depending on the sample. Table 1 provides the specific PXCT imaging parameters for each sample. The β and δ parts of the reconstructed data were observed to provide the same information, but with lower noise in the δ values, and so the β part was discarded.
Data obtained from PXCT experiments was processed in Avizo 9.5 for quantitative analysis and 3D visualization. An important step to reach this goal is the segmentation of materials of interest, i.e. dividing the data array into materials zones based on their δ-value (which correlates closely with electron density when the X-ray energy is not close to an elemental resonance67). The most interesting materials in Zwischgold samples are Au and Ag, the main Ag corrosion products such as Ag2S and AgCl, and materials expected to be present in the varnish coating and bole substrates. Quartz (SiO2), kaolinite (Al2Si2O5(OH)4, Na2SiO3, Mg3Si4O10(OH)2) and calcite (CaCO3) are main bole materials.68 The earth pigments red ochre (main component hematite Fe2O3) and yellow ochre (main component goethite FeO(OH)) were commonly mixed with bole materials to make red and yellow boles. Other materials that are expected to be observed include amorphous carbon and aluminium as protective and conductive coatings, as well as gallium which was used as the FIB ion source. The δ and β values for 8.7 keV photons interacting with materials of interest in Zwischgold samples were calculated using the atomic scattering factors from Henke et al.67 and presented in Table S1 in the ESI.†
R. H. F. acknowledges funding by the BMBF under contract 05K19WE2 and the Deutsche Forschungsgemeinschaft within GRK 1896. E. H. R. T. was supported by the Swiss National Science Foundation (SNSF) grant numbers 200021_152554 and 200020_169623. The research also used resources of the Centre for Functional Nanomaterials (https://www.sciencedirect.com/topics/engineering/nanomaterials), which is a US DOE Office of Science Facility, at Brookhaven National Laboratory under Contract No. DE-SC0012704. Part of this work was performed at the DFG-funded Micro-and Nanoanalytics Facility (MNaF) of the University of Siegen.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2nr03367d |