Burcin Izbudak†
a,
Berivan Cecen†bcd,
Ingrid Anaya†e,
Amir K. Miribc,
Ayca Bal-Ozturk*af and
Erdal Karaoz*agh
aDepartment of Stem Cell and Tissue Engineering, Institute of Health Sciences, Istinye University, Istanbul, Turkey. E-mail: aycabal@gmail.com; ekaraoz@istinye.edu.tr
bBiofabrication Lab, Department of Mechanical Engineering, Rowan University, Glassboro, NJ 08028, USA
cSchool of Medical Engineering, Science and Health, Rowan University, Camden, NJ 08103, USA
dDepartment of Molecular Biology and Genetics, Faculty of Engineering and Natural Sciences, Istinye University, 34010, Zeytinburnu, Istanbul, Turkey
eDepartment of Bioengineering, Tecnológico de Monterrey, Campus Monterrey, CP, 64849, Monterrey, Nuevo León, México
fDepartment of Analytical Chemistry, Faculty of Pharmacy, Istinye University, Istanbul, Turkey
gDepartment of Histology and Embryology, Faculty of Medicine, Istinye University Istanbul, Turkey
hCenter for Regenerative Medicine and Stem Cell Research and Manufacturing (LivMedCell), Istanbul, Turkey
First published on 9th September 2021
Layered double hydroxides (LDHs), when incorporated into biomaterials, provide a tunable composition, controllable particle size, anion exchange capacity, pH-sensitive solubility, high-drug loading efficiency, efficient gene and drug delivery, controlled release and effective intracellular uptake, natural biodegradability in an acidic medium, and negligible toxicity. In this review, we study potential applications of LDH-based nanocomposite scaffolds for tissue engineering. We address how LDHs provide new solutions for nanostructure stability and enhance in vivo studies' success.
Fig. 1 (A) The general structure of LDHs. This figure is reproduced from ref. 19 with permission from Elsevier, copyright 2017. (B) The available design of LDHs experiments. This figure is reproduced from ref. 15 with permission from John Wiley and Sons, copyright 2019. (C) Current research on LDHs, and the existing category of LDH precursors, nanoparticles, hybrids, and biohybrid composites. This figure is reproduced from ref. 24 with permission from John Wiley and Sons, copyright 2017. |
Different characterization methods were used to study LDHs with biological components, as shown in Fig. 1B and C.15,24 The three main groups of LDHs used in biomedical applications are (I) organic agents entrapped between the interlayer of LDHs, (II) the dispersion of LDHs into a polymeric network, and (III) LDHs intercalated with biological molecules.25 There have been numerous studies on these three groups, such as bone tissue engineering;26 however, there are limited tissue engineering studies. Here, we introduced the potential applications of LDHs in tissue engineering applications. We focus on biocompatibility, antibacterial properties, and osteogenic differentiation associated with LDHs in tissue engineering, and we discuss current challenges and future perspectives. The manuscript is divided into four sections. First, the bioactivity of LDHs in different systems is discussed. Second, the efficiency of LDHs for antibacterial properties is well explained for various cases. Third, their applications in bone engineering are shown in detail. Lastly, future trends and perspectives are discussed. In this paper, we introduce the recent advances of LDHs for bone and cartilage tissue-engineered scaffolds in regenerative medicine as drug delivery carriers.
LDH type/molar ratio | Size (nm) | Conc. (μg mL−1) | Cell types | Assay (test) | Results | Ref. |
---|---|---|---|---|---|---|
Mg–Al LDHs 2:1 | 50–100 | 40 | Human embryonic kidney cells (293T) | MTT | The non-toxic effect, more than 80% viability after three days | 31 |
Zn–Al LDHs 2:1 | — | 5–150 | Mouse fibroblast cells (3T3) | MTT | 90% viability at 100 μg mL−1 concentration | 32 |
Mg–Al LDHs 3:1 | 80–90 | 20 | Human cervical cancer | MTT | Very low toxicity after 72 h treatment | 33 |
Mg–Al LDHs 4:1 | — | 50 | Breast (MCF-7), HeLa, and fibroblast (3T3) cells | MTT | Non-toxic effect | 34 |
Mg–Al LDHs 3:1 | — | 40 | GES-1, MKN45 and SGC-7901 cells | MTT | Non-toxic effect | 35 |
Zn-LDHs | — | 25–0.195 | Monkey kidney (Vero-3) cells | MTT | 92% viability at 25 μg mL−1 concentration | 36 |
Zn-LDHs | — | 5–500 mg kg−1 | Rat | Oral toxicity | Non-clinical toxicity and animal demise at 5–500 mg kg−1 dose | 37 |
Zn–Al LDHs 2:1 | — | 25–800 | PC12 cells | MTT | Low toxic effect at 800 μg mL−1 concentration | 38 |
Mg–Al LDHs 3:1 | 100 | 2–40 | Mouse embryonic stem cells (mESC) | MTT | Excellent biocompatibility | 39 |
Mg–Al LDHs 3:1 | 50, 100 | 10–400 | Mouse embryonic stem cells (mESC) | MTT | No significant cytotoxicity at a concentration up to 40 μg mL−1 | 40 |
Mg–Al LDHs 2:1 | — | 1–1000 | Human leukemia cells (HL-60) | MTT | Non-toxic effect | 41 |
Bioadhesion is another critical consideration in designing hydrogels for tissue regeneration. The hydrogels' tight adhesion potentially leads to better integration with the surrounding biological tissues, facilitating infiltration of bioactive molecules and cells promoting tissue healing.27 The cellular and biochemical properties of LDHs were evaluated, in which two combinations of LDHs (Mg–Al–Cl and Zn–Al–Cl) with different concentrations were tested (Fig. 2A). Standard viability analysis (MTT) was performed to assess the acceptable range of concentrations. A range of 0.002–0.2 mg mL−1 did not lead to a half-maximal inhibitory concentration (IC50) value within 24 h. Mg–Al–Cl showed a better cell growth pathway for fibroblast adhesion when compared to Zn–Al–Cl (Fig. 2B and C). The effects of the culture media on the shape of LDHs were stated to be negligible. The results indicate that LDHs guide cellular adhesion, migration, proliferation and delineate new advances on the biomaterial area implemented for soft tissue bioengineering.26 Baek et al. examined the cytotoxic effects of two different types of LDHs, Mg–Al–CO3, and Mg–Al–Cl, on human lung alveolar carcinoma epithelial cells (A549) and normal human lung alveolar epithelial cells (L-132). They prepared LDHs by the molar ratio of Mg/Al = 2 using the co-precipitation process. The production of reactive oxygen species (ROS) was then determined with a cell permeable fluorescent probe, 2′,7′-dichlorofluorescein diacetate (H2DCFDA). The human lung alveolar carcinoma epithelial cells (A549) and normal human lung alveolar epithelial cells (L-132) were treated with LDHs at concentrations up to 1000 μg mL−1 for 72 hours. The stability and toxicity of LDHs were investigated for the effect of the proliferation of L-132 and A549 cell lines. Mg–Al–CO3 LDHs with a size of 200 nm led to significant ROS in the A549 cell line. Mg–Al–CO3 LDHs showed higher toxicity in comparison to Mg–Al–Cl LDHs.28
Fig. 2 (A) The LDHs structure. (B) The effect of two compositions and types of LDHs, Mg–AI–CI and Zn–Al–CI LDHs, on fibroblast adhesion. (C) The cell morphologies on the LDHs constructs after 24 hours. This figure is reproduced from ref. 26 with permission from John Wiley and Sons, copyright 2019. |
Choi et al.29 evaluated the toxicity of anionic clay, layered metal hydroxide nanoparticles, two human lung epithelial cells, and carcinoma A549 normal L-132 cells. They determined it to be low tested at the concentrations used (<250 μg mL−1) within 48 h in comparison with other inorganic nanoparticles, such as silica, iron oxide, and carbon nanotubes. Higher concentrations (250–500 μg mL−1) of LDHs for 72 h resulted in an inflammatory response with oxidative stress and membrane damage. Therefore, oxidative stress can be caused depending on the type of nanoparticle,30 concentration, and exposure time, affecting the toxicity.
Peng et al. developed the different LDHs (Mg–Al, Mg–Fe, Zn–Al, and Zn–Fe) to apply bone implants. They evaluated the feasibility of the LDH with biological functional elements as bone implants, M2+ was chosen for being essential for bone regeneration, Zn2+ was selected for skeletal development and antibacterial activity, while Al3+ and Fe3+ for their low toxicity. Osteoblast-like cells (MC3T3-E1), related to bone growth, and human umbilical endothelial cells (HUVECs) were investigated to determine the cytotoxic activity LDHs. LDHs with specific amounts in the form of extracts or suspensions were treated. Mg–Al and Mg–Fe LDHs indicated higher cell viability than Zn–Al and Zn–Fe LDHs. The concentrations of Zn–Al LDHs extract higher than 1.11 mg mL−1 led to significant toxicity. The apparent toxicity of Zn–Fe LDHs was observed at an extract concentration of 123.5 μg mL−1. Unlike the extract, Zn–Al and Zn–Fe LDHs suspensions showed more severe toxicity to HUVEC and MC3T3-E1 than Mg–Al Mg–Fe LDHs when the concentration of their breaks was higher than 41.2 μg mL−1.42 The present study evaluated the mechanical properties, as well as cytotoxicity and antibacterial ability. Zn–Fe LDHs is the most suitable for a bone implant. It has the highest hardness and elastic modulus; a mismatch in the elastic modulus between the bone and the implant would lead to stress shielding, which causes bone resorption after surgery.
One major issue of bone implants is the formation of bacteria films. Thus, it is essential to engineer the LDHs with antibacterial potential to allow their osseointegration. It has been reported in the literature that Zn damages the membrane and nucleic acid and denatures the bacteria proteins and enzymes. Therefore, bacteria (E.coli and S. aureus) showed lower tolerance concentration of Zn–Al LDH and Zn–Fe LDH. Soo et al. reported that Mg–Al and Zn–Al LDHs at concentrations up to 500 μg mL−1 had no toxic effects within 48 hours in various cell lines and red blood cells.
The findings revealed that Zn–Al LDHs induced much more serious membrane damage and hemolysis than Mg–Al LDHs. Based on these findings, Mg–Al LDHs in various sizes (50, 100, 200, 350 nm) were tested. Mg–Al LDHs at concentrations up to 500 μg mL−1 were treated with A549 cells for 48 hours. While Mg–Al LDHs of 50 nm in size treated with A549 cell lines were found to be more toxic than larger nanoparticles, Mg–Al LDHs in size range from 100 to 200 nm were found to show very low cytotoxicity. Even LDHs of 50 nm in size, which is a toxic effect in vitro, did not result in body weight loss or mortality in vivo. On the other side, in in vivo studies, all LDHs groups did not cause any mortality or weight loss of 600 mg kg−1. The assumption that LDHs are attractive biocompatible biomaterials for biological and medical applications has been confirmed.43
Cunha et al. (2016) assessed the biocompatibility, biointegration, non-immunogenic feature, and antigenicity properties of Mg–Al and Zn–Al LDHs tablets post-implanting intramuscularly in rat abdominal as it allows to test the activation of the whole immune response in few 7 days and the rejection process by fibrous capsule formation in a more extended period, 28 days through the microcirculation.44 A stroboscopic LED video-microscopy was used to observe the micro-circulation patterns of the host tissues around LDHs. The two types of LDHs had 80–100 nm, and the co-precipitation process produced them. The sterilized LDHs were implanted in rats' abdominal walls, and the results showed that LDHs had appropriate biocompatibility on day 7. Histological tests evaluated the reaction of the LDHs with host tissue post-implantation neo-vascularized connective tissue was observed around the treated area (Fig. 3). The real-time observation showed that muscle tissues implanted with Mg–Al and Zn–Al LDHs support non-immunogenic properties, adequate extracellular matrix remodeling to the desired collagen type wound healing according to the tablet biophysical composition. This healing process involves the deposition of collagen and fibronectin fibers; the Zn–Al LDH tablet sample exhibited a predominance of collagen type-III fibers. Besides, the alkaline pH buffering behavior of the LDHs promoted normal cellular response as chemotaxis, respiratory activity, and proliferative capacity of leukocytes; thus, good tissue repair response. These results suggest that they can be used in biomedical applications for drug delivery.44
Fig. 3 Histological images of the implants after 28 days show the final tissue reconstruction and the persistence of the implanted LDHs constructs. This figure is reproduced from ref. 44 with permission from Springer Nature, copyright 2016. |
Nanocomposite-based hydrogels are enhancing the mechanical and chemical properties of hydrogels and expanding their biomedical applications. When encapsulated with inorganic nanoparticles, they have shown excellent biocompatibility, stability, and mechanical properties compared to new hydrogels due to the remarkable physical, chemical, and biological features of inorganic nanoparticles. Wang et al. mixed LDHs and nanohydroxyapatite (HAp) to develop a porous nanocomposite hydrogel made of poly(N-isopropyl acrylamide) (PNIPAm/LDHs/HAp), which showed superior hemocompatibility, enhanced mechanical strength, and reversible swelling/deswelling properties. These results support that the developed hydrogel embedded with LDHs and HAp has excellent potential for tissue engineering and clinical practices.45
Fig. 4 (A) A schematic illustration of an antibacterial-experimental strategy and possible antibacterial mechanism of LDHs. This figure is reproduced from ref. 50 with permission from Elsevier, copyright 2020. (B) Effects of CS, Zn–Al LDHs, and CS/Zn–Al LDHs against P. cyclopium and E. coli. This figure is reproduced from ref. 52 with permission from MDPI, copyright 2019. |
LDHs also show strong ion-exchange potential and porous structures; for example, Zn ion-based LDHs exhibit strong antibacterial properties leading to bone implant's fast regeneration.51 Peng et al. have recently reported an alternative method by preparing Mg–Al, Mg–Fe, Zn–AI, and Zn–Fe LDHs. Extract and suspension forms of Zn–Al LDHs and Zn–Fe LDHs displayed a better antibacterial impact on Gram-positive S. aureus and Gram-negative E. coli compared to the Mg–Al and Mg–Fe LDHs. Zn–AI and Zn–Fe LDHs into the scaffold showed higher success and potential for the application of antibacterial implants.42 The bacterial resistance to antibiotics increases over time. Gohi et al. developed a new organic–inorganic hybrid biomaterial consisting of Zn–Al LDHs/chitosan (CS). With the release of Zn2+ and Al3+ metal ions from Zn–Al LDHs/CS hybrid biomaterial, an increase of the inhibition zone of 41.6% against E. coli and almost 100% for Penicillium cyclopium (P. cyclopium) was observed (Fig. 4B).52 In another study, an antibacterial environmentally friendly polyurethane (WPU)-based composite was synthesized with Zn–Al LDHs, and ZnO, ZnO LDHs have been reported to inhibit bacteria growth and their proliferation effectively. The antibacterial effect was assessed for composite biomaterials against Gram-negative E. coli and Gram-positive S. aureus. The results show that WPU embedded with ZnAl-LDHs/ZnO has solid antibacterial potential. The antibacterial activity of WPU/Zn–Al LDHs/ZnO composite exists on two mechanisms. First, ZnO activates intercellular ROS such as hydrogen peroxide (H2O2) and strengthens oxidizing agents, damaging the bacterial cells. Second, Zn+2 ions in LDHs penetrate the bacterial membrane while altering the cell membrane's permeability and causing individual proteins' denaturation.53 In another similar study, the proliferation of S. cerevisiae, S. aureus, and E. coli has been severely inhibited by Zn–Ti LDHs and evaluated the size-dependent antibacterial behavior of Zn–Ti LDHs. Ti+3 cations in Zn–Ti LDHs with a size of 40 nm showed a more active antibacterial effect than metal oxide and TiO2. Zn–Ti LDHs killed more than 95% of the bacteria and exhibited excellent antibacterial action.54
Since silver has antibacterial properties, composite biomaterials have been preferred in many studies. Mehdi et al. focused on the antibacterial effect of silver and LDHs in the carboxy-methyl-cellulose (CMC)-based hydrogel. CMC nanocomposites' antibacterial effect includes Mg–Al, Ni–Al, Zn–Al, and-Al LDHs against E. coli and S. aureus bacteria has been investigated. Cu–Al LDHs/CMC and Zn–AI LDHs/CMC nanocomposites showed more antibacterial effects than nanocomposites, including Mg–Al Ni–Al LDHs. This is because of Cu and Zn ions' antibacterial properties released from Cu–Al LDHs/CMC and Zn–AI LDHs/CMC constructs. The inhibition zone for Cu–Al LDHs/CMC and Zn–Al LDHs/CMC against E. coli decreased after 3 days. On the other hand, they displayed better potential towards S. aureus and kept their antibacterial impact for more than 2 weeks.55 Gabriela et al. reported the antibacterial effects on Zn–AI LDH, Ag/Zn–AI LDHs, and AgNP against S. aureus and E. coli. The superior stability and efficacy of the antibacterial potential of Ag/Zn–AI LDHs are possibly owing to the power of the LDHs structure to adsorb microorganisms; thus, enabling strong interactions with the silver from the surface.56
Ahmed et al. successfully used Zn for antibacterial properties of polyaniline (PAn) nanocomposite, including Zn–Al LDHs. The antimicrobial activity of PAn/Zn–Al LDHs nanocomposites was assessed against Gram-positive (Staphylococcus aureus), Gram-negative (Pseudomonas aeruginosa) bacteria, and fungi (Candida albicans). The results reported that PAn/Zn–Al LDHs prevented bacteria and fungi from stuck on the surface and provided antimicrobial effects by growing the ability.57 In another study, Penicillin G (PNG)-loaded Zn–Al LDHs prepared to make prolonged antibacterial potential against E. coli. In the meantime, the released Zn+2 ions from Zn–Al LDHs had an antibacterial ability by significantly improving the antibacterial effect of PNG.58
Jin et al. intercalated an anticancer drug 5-fluorouracil/cyclodextrin (5-FU/CMCD) into a Zn–Al LDH. The drug release time was prolonged and controlled by the hydrophobic environment of the CMCD cavity and by the durability of the LDH. Therefore, the release behavior of 5-FU from 5-FU/CMCD-LDH composite could be modulated by a change in the environmental pH value.1 Other pharmaceutical compounds such as ibuprofen, fenbufen, and diclofenac have been incorporated into LDHs and exhibited LDH-based tunable drug delivery systems' feasibility.1,9,19
LDH type | Application | Cell line/tissue model | Results | Ref. |
---|---|---|---|---|
Mg–Al, Mg–Fe, ZN–Al, and Zn–Fe LDHs | Bone implantation | MC3T3-E1 | Zn–Fe had the highest hardness and elastic modulus, most suitable avoiding bone resorption after surgery. | 42 |
Mg–Fe LDH | Bone implantation | rBMSCs | Mg–Fe LDH films on titanium increased the ALP activity, collagen secretion, ECM mineralization, and proliferation and osteogenic differentiation. | 70 |
Cs/Ag-laden MgSrFe LDHs | Bone regeneration | hBMSCs | ALP, RUNX2 and BMP-2 expression increased. Ag and Sr elements supported osteogenic differentiation and bone formation. | 66 |
PD-LDHs | Bone regeneration | hMSCs | Increased the mechanical strength, bioadhesion, spreading and osteogenic differentiation of hMSCs. | 67 |
Mg–Al LDHs | Bone regeneration | rBMSCs and MC3T3-E1 | Mg–Al LDHs and titanium's alkaline environment regulated the oxidative stress, proliferation, and ALP activities of osteoblast cells. | 63 |
CS/Mg–Al LDHs/PFT-α | Bone regeneration | hBMSCs | PFT-α induced the GSK3-β/y-cantenin pathway and showed an enhancing effect on hBMSC differentiation. | 71 |
Mg–Al and Zn–Al LDHs | Bone regeneration | Preosteoblasts | Enhanced osteocalcin (OCN), RUNX2, and Osterix (OSX). Reprogramming the mineralization and osteoclast-osteoblast fusion. | 61 |
Vitamin D3 (VD3) LDH-Hap | Bone regeneration | HAp containing scaffolds (LHG and LHGD) | Increased mechanical strength and ossification. | 73 |
(PAEU/LDH/hGH)Adenosine (Ado)-loaded Mg–Al LDHs | Bone regeneration | HCT-166 cell lines and in vivo rat model | Osteogenic differentiation of stem cells through the activation of the adenosine a2b receptor. Repaired rat tibia after six weeks. | 68 |
Bis-GMA and TEGDMAwith Mg–Al–F LDH | Dental applications | hDPSCs | Fluoride release increased the hDPSCs and ALP activity, an odontoblastic differentiation. | 61 |
Mg–Al LDHs | Tissue regeneration and drug release | Calvarial osteoblasts isolated from mice | High ALP potential and bone nodule, Mg–Al LDHs supported anti-inflammatory and osteogenic activity. | 62 |
PAG-PA-PD with Mg–Al LDHs | Chondrogenic differentiation | TMSCs | Increased mRNA ad protein levels of type II collagen and SOX9 in TMSCs | 65 |
The microstructure and chemical composition of gelatin/LDHs/Hap-based scaffolds were similar to native bone structures. The gelatin/LDHs/HAp-based scaffold's bone regeneration ability was shown in orthopedic and regenerative surgery for bone healing.65 For significant bone defects to restore healthy bone, engineered scaffolds should be biocompatible and support osteogenic differentiation without causing infection. Dandan et al. successfully prepared a new nanocomposite scaffold by combining Ag-laden MgSrFe LDHs with CS (CS/Ag-MgSrFe LDH). CS/Ag-MgSrFe nanocomposite scaffold was non-toxic on human bone marrow-derived mesenchymal stem cells (hBMSCs). The cells showed enhanced spread, proliferation, and adhesion on the scaffold. Due to the release of Sr2+ ions from LDHs, ALP RUNX2 and BMP-2 expression increased. CS/Mg–Fe LDHs were compared with CS/Ag-MgSrFe LDH nanocomposite scaffold, and data indicated that the nanocomposite scaffolds containing Ag and Sr elements support osteogenic differentiation. Besides, Ag components in LDHs provided excellent bone formation, which gained antibacterial activity and kept osteoinductivity (Fig. 5C).66
Fig. 5 (A) Schematic illustration of polydopamine coating on LDHs and nanocomposite scaffold prepared by using 4-arm thiol-terminated polyethylene glycol (4-arm PEG-SH) and polydopamine-coated LDHs (PD-LDHs), which can carry biomacromolecules and act as the sealant for bone fracture. (B) The prepared nanocomposite scaffold has a strong sealant function for fractured bone pieces. This figure is reproduced from ref. 67 with permission from John Wiley and Sons, copyright 2016. (C) Alizarin Red staining for ECM mineralization of hBMSCs with CS/Mg–Fe, CS/Ag–MgFe/, CS/MgSrFe, and CS/Ag-MgSrFe scaffolds. This figure is reproduced from ref. 66 with permission from John Wiley and Sons, copyright 2017. (D) The cranial defect was created, and CS/LDHs-PFTα or CS/LDHs constructs were placed in the cranial defects. (E) After twelve weeks, the defect region was examined using reconstructing micro-CT images. This figure is reproduced from ref. 71 with permission from RSC Pub, copyright 2017. |
Heqin et al. utilized a new nanocomposite consisting of PEG-based hydrogel by using polydopamine-coated LDHs (PD-LDHs). The catechol-rich PD-LDHs nanosheets not only possessed strong bioadhesive properties in the aqueous environments but also increased the mechanical strength of the obtained PEG-based hydrogel (Fig. 5A and B). It was seen that PD-LDHs cross-linked PEG-based nanocomposite hydrogel enhanced adhesion, spreading, and osteogenic differentiation of human derived mesenchymal stem cells (hMSCs). As a result, they carried out a nanocomposite hydrogel that can have incredible potency in regenerative medicine and open up a new way to design PEG-based nanocomposite constructs.67
Loredana et al. have explored the fundamental effects of fluoride ion-doped Mg–Al LDHs into hydrogel scaffolds. Bisphenol-A glycidyl dimethacrylate (Bis-GMA) and tri-ethylene glycol dimethacrylate (TEGDMA) combined with Mg–Al–F LDH. The addition of Mg–Al–F LDHs promoted the mechanical features of the hydrogel resin. Slow fluoride release from hydrogel increased human dental pulp stem cells (hDPSCs) and ALP activity, an early odontoblastic differentiation for 28 days. Considering these results, Mg–Al–F LDHs can be used as a dental filler for tooth resins.68 In another study, Michelle et al. developed a guided tissue regeneration membrane suitable for periodontology. The controlled release of drugs was achieved from tetracycline and alendronate from Mg–Al LDHs into the poly(lactic-co-glycolic acid) (PLGA)-based membranes. Calvarial osteoblasts isolated from mice were incubated with membranes for five weeks. A high ALP potential and bone nodule formation were detected, and Mg-AI LDHs supported anti-inflammatory and osteogenic activity as a bone graft.69
Tan et al. have designed a biomaterial to capture implant failures to investigate antibacterial and osteogenic activities on the different alkaline microenvironment of titanium surface-associated with Mg–Al LDHs. Cellular adhesion, proliferation, and ALP activities were examined on rat bone marrow mesenchymal stem cells (rBMSCs) and mouse osteoblast cells (MC3T3-E1) 1,4 and 7 days. They also confirmed that Mg-AI LDHs and titanium's alkaline environment regulates the oxidative stress, proliferation, and ALP activities of osteoblast cells.63 In another study, Qianwen et al. produced Mg–Fe LDH films on titanium surfaces for challenging tissue implantation. Biocompatibility, proliferation, and osteoblast differentiation of the films were investigated on rBMSCs. They noticed that Mg–Fe LDH films on titanium increased the proliferation and osteogenic differentiation, ALP activity, collagen secretion, and ECM mineralization of rBMSCs, representing the encouraged applications as hard tissue implant materials.70
p53 has a key rol in bone formation and metabolism. Scientists have recently reported that decreased p53 function is associated with bone formation. Pifithrin-α (PFT-α) is a chemical inhibitor of p53 that prohibits p53 role for bone formation.72 Yi-Xuan et al. investigated the different doses of PFT-α on the CS/Mg–Al LDHs composite scaffolds (CS/Mg–Al LDHs/PFT-α) hBMSCs. They claimed that CS/Mg–Al LDHs/PFT-α scaffolds could be a novel strategy with natural bone regeneration functionality. For all that, they emphasized the increased COL1, β-catenin, and p53 by inducing the GSK3β/y-catenin pathway due to the release of PFT-α. Consequently, PFT-α induced the Wnt/β-catenin pathway and showed an enhancing effect on hBMSC differentiation (Fig. 5D and E).71 In another study, the molecular mechanisms of Mg–Al and Zn–Al LDHs from preosteoblast to mature osteoblast led to enhanced osteocalcin (OCN), RUNX2, and Osterix (OSX). Mg–Al LDHs have a keynote regulation on OSX mRNA levels reprogramming the mineralization and osteoclast-osteoblast fusion balance with signal molecules.61 Fateme et al. investigated the encapsulation of vitamin D3 on the gelatin-based scaffolds. LDH-HAp was combined with vitamin D3 to reinforce scaffolds. They observed that vitamin D3 plays a primary function in calcium accumulation, ALP activity regulation and osteoblastic expression. Reinforcement with vitamin D3 (VD3) the LDH-HAp into the scaffolds increased the mechanical strength and ossification, mimicking the mineral/organic structure of the natural bone and VD3 signaling effect. The HAp containing scaffolds (LHG and LHGD) avoided the adverse impacts of burst release, showed less water uptake, and recrystallized HAp, resulting in more bioactivity in these scaffolds. The more packed structures of LGD and LHGD lead to a decrease in the degradation rate due to less diffusion.73
Narendra et al. have prepared nano-bio hybrid injectable scaffolds (PAEU/LDH/hGH) to reduce the adverse effects of human growth hormone (hGH) inhibited by their early degradation short half-life. hGH was intercalated in the positively charged Mg–Al LDHs through an anion exchange technique (Fig. 6B). The injectable nano-biohybrid scaffold showed the delayed-hGH release diffusion by dual-ionic interactions as the scaffolds' pH and temperature sensitivity. Cytotoxicity using HCT-166 cell lines and in vivo rat model was used to study the scaffolds' biological response.74
Fig. 6 (A) In vivo implantation of gelatin/LDHs/HAp-based scaffold for bone tissue engineering application. This figure is reproduced from ref. 17 with permission from Elsevier, copyright 2017. (B) Schematic hGH loading in LDHs, and nanocomposite hydrogels. This figure is reproduced from ref. 74 with permission from RSC Pub, copyright 2015. (C) Schematic representation of Ado-loaded Mg–Fe LDHs preparation and their applications. The developed nanoparticular platform synergistically induces the osteogenic differentiation of stem cells for healing of extended bone defects by co-delivering the Ado ligand and ligation stimulator (Mg ion). This figure is reproduced from ref. 64 with permission from Elsevier, copyright 2017. |
Injectable hydrogels loaded with LDHs-hGH may be used effectively for sustained-hGH delivery to enhance biological efficaciousness and patient compliance.74 Adenosine (Ado)-loaded Mg–Fe LDHs were also embedded within the injectable hydrogel to support the bone defect healing (Fig. 6C). The dual delivery of Ado and Mg ions from Ado-loaded Mg–Fe LDHs containing injectable hydrogel supported osteogenic differentiation of stem cells through the synergistic activation of the adenosine A2b receptor was indicated. Furthermore, the injectable hydrogel promoted repairing rat tibia bone defects after six weeks. The serum hGH concentration remained high (∼1 ng mL−1) with the LDH-hGH complex and pristine PAEU-hGH hydrogel for 1 and 3 days respectively, with a minimal initial burst release compared with hGH alone; these effects are mainly attributed to the formation of ionic complexes between the anionic hGH and cationic PAEU hydrogels and the smaller interconnected pores in the hydrogel.75
Fig. 7 2D/3D nanocomposite platform incorporating stem cells, kartogenin (KGN), and RGD-coated LDHs in a poly(ethylene glycol)-poly(L-alanine)-poly(L-aspartate) (PEG-PA-PD) triblock copolymer thermogel for effective chondrogenic differentiation of the stem cells. This figure is reproduced from ref. 76 with permission from American Chemical Society, copyright 2017. |
Giriprasath et al. developed a novel double-layer scaffold made of HAp pellets coated by poly(3-hydroxybutyric acid)-poly(N-vinylpyrrolidone) matrix and LDHs (HAp: NFM-LDHs). The nanofibrous bone graft's in vitro biocompatibility, and fluorescent activity were examined for 1, 3, 7, and 14 days. MG63 cells showed outstanding cell adhesion and proliferation on both the top and bottom layers of the scaffolds. The nanofibrous matrix resulted in significantly higher cell adhesion from day 3 to 14. Compared to the control of LDHs in the structure, cell adhesion increased significantly on HAp: NFM-LDHs surface. This approach provides the opportunity to perform alternative nanofibrous bone grafts containing Mg–Al LDHs for bone tissue engineering applications.77 Hsiao et al. indicated the possibility that an injectable and thermoresponsive hydrogel would be suitable for gene therapy by using osteoarthritic chondrocytes. They formulated poly(N-isopropylacrylamide) (pNIPAAM) hydrogels with Mg–Al or Mg–Fe LDHs by encapsulating siRNA and providing 80–95% siRNA transfection in PNIPAAM/LDHs hybrid hydrogels. Expressions of ACAN, MMP13, Col2A1 genes have been observed. Hydrogels in blend with LDHs may be good candidates specifying both cell delivery and siRNA transfection.78
Seyedeh et al. have created a new fiber-based biomaterial that can mimic ECM in tissue organ development and regeneration. They combined samples with Mg–Al LDHs ranging from 0.1 wt% to 10 wt% in in vitro experiments with stem cells derived from mouse adipose (mADSCs). They also assessed the effects of mADSCs on adhesion, proliferation, and viability, and adipogenic differentiation throughout PCL enrichment with Mg–Al LDHs. The composite electrospun PCL scaffolds had a better cell adhesion and proliferation compared to non-treated PCL. Additionally, a substantial increase in the adipogenic differentiation of mADSCs was obtained. The PCL-LDHs scaffolds with high porosity (94%) indicated numerous possibilities in applying soft tissue engineering.79
Due to the complication of the corneal stroma ultrastructure, efficient ECM production is exceptionally challenging. Mojgan et al. have created a new poly(urethane-urea) (PUU) based scaffold that can be used in corneal tissue engineering. Zn–Al LDHs were synthesized using the co-precipitation method, laden with vitamin C (VC), and dispersed in the PUU to control VC release. The scaffolds were prepared with electrospinning to mimic the corneal stroma. VC-loaded Zn–Al LDHs allowed the adhesion of the corneal regeneration. According to the in vitro effects of three types of experimental groups (PUU, PUU/Zn–Al LDHs, and PUU/VC/Zn–Al LDHs), stromal keratocyte cells exhibited some level of proliferation on the scaffolds through the peak value obtained with PUU/VC/Zn–Al LDHs scaffolds after one week. The results showed significant differences in gene expression. A specific increase was observed in the expression of ALDH3A1 protein, the keratocyte marker, and the expression of ACTA2 gene α-SMA protein of the myofibroblast phenotype, the sustained release of VC from PUU/VC/Zn–Al LDHs scaffolds. All results suggest that PUU/VC/Zn–Al LDHs scaffolds may be ideal for corneal stromal tissue engineering.80
Stimuli-responsive nanomaterials have been developed for delivering the drug to tumors. In the tumor hypoxic environment LDHs react with H2O2, this leads to a change in their structure and then the release of the drug improving the therapeutic efficacy. In the future, LDHs enhanced with nanoparticles could potentially be used in a lower pH medium for faster and accurate tumor target drug delivery. Despite the increase of LDHs applications in cancer research, it is still required to understand LDHs and cells' interaction mechanisms fully. Further studies are required for understanding the activation of the intracellular pathways of the cancer cells and tumor cell apoptosis with the help of the LDHs. Moreover, proteins and antigens could be delivered by LDH nano-vaccines for cancer immunotherapy and to enhance the immune system overall. Another major highlight of the LDHs is their efficacy in delivering genes to the target site. They have been shown capable of transporting DNA and RNA avoiding non-specific sites, some authors suggest that LDHs could be used for transfection methods. Also, organic molecules such as hormones and vitamins can be loaded into the LDHs for controlled release.
Many challenges still exist for LDHs to evolve as a drug delivery system of choice. While the thermosensitive LDHs can be used for anti-HIV drug delivery in the vagina tract, the positively charged LDHs can be a strategy for ocular drug delivery, and its pH-dependent degradation can be a better approach for tumor-targeted drug delivery; the sensitivity of LDHs in an acidic environment is a hurdle in oral drug delivery due to the enzymatic and acidic degradation in the stomach and less absorption from the small intestine, this could be prevented by using polymer coating or other encapsulation methods. Moreover, when administered via the blood system they may interact with negatively charge biomolecules in the environment that may lead to loss of surface charge, aggregation, and precipitation, thus, improvement of the LDHs stability is a major challenge. Despite the advances in the modification or functionalization of the surface of the LDHs for major stability, there are a few reports in drug delivery applications. Further studies are required to understand the in vivo biodegradability and clearance of LDHs nanomaterials and to include development of ultra-thin LDH nanosheets to avoid pre-mature therapeutic agents release and controlled drug release.
LDHs have been used as composites for regenerative medicine and tissue engineering applications. Herewith, LDHs can create a bio-safe environment around cells and tissue surfaces. It is expected that tissue scaffolds should be mimicked like ECM for cell adhesion, intercellular interaction, and cell differentiation during tissue repairing. The absence of infection is essential to accelerate the tissue regeneration in these tissue implants. Thus, the scaffolds' mechanical properties can be tuned by using LDHs to obtain a favorable environment as successful implants with the antibacterial properties of LDHs. Moreover, in bone therapy and regeneration, the release of Mg+2 ions from Mg–Al LDHs, provides an alkaline environment formation and activation of osteogenic differentiation pathways. Furthermore, Mg–Al LDHs can also induce ALP activation of osteoblasts. In the future, to develop the best commercialization for LDHs-based biomaterials in clinic, it is necessary to improve the surface modification, the drug loading, and the synthesis methods to produce highly stable and uniform LHDs with minimal variation in size, geometry, and thickness.