Suman
Chhetri
*a and
Tapas
Kuila
*bc
aDepartment of Mechanical Engineering, College of Engineering, University of Hawaii at Manoa, Honolulu, 96822, USA. E-mail: chhetri@hawaii.edu; chhetrisuman86@gmail.com; Tel: +1-808-8078-144
bElectric Mobility & Tribology Research Group, Council of Scientific and Industrial Research-Central Mechanical Engineering Research Institute, Durgapur, 713209, India. E-mail: tkuila@gmail.com
cAcademy of Scientific and Innovative Research (AcSIR), CSIR-Human Resource Development Centre, (CSIR-HRDC) Campus, Postal Staff College Area, Sector 19, Kamla Nehru Nagar, Ghaziabad, 201002, Uttar Pradesh, India
First published on 23rd April 2024
Secondary electromagnetic pollution generated due to the inevitable reflection in solid/thin film conducting polymer composites has been a major barrier in realizing high-performance absorption-dominated electromagnetic interference (EMI) shielding. In the past, prodigious efforts were made to minimize the reflection by tailoring the impedance characteristics between the air and the substrate. For instance, incorporation of a microcellular scaffold (3D structure) such as foam and aerogel in a polymer matrix have been extensively investigated to tailor the surface impedance matching and achieve enhanced absorption. To date, application of the 3D graphene microcellular scaffold alone or its hybrid with other magnetic, conductive, and dielectric materials has been continuously pursued to diminish reflectivity and increase absorption via the dielectric and interfacial relaxation loss mechanism. An aerogel and foam structure contains multiscale pores (micro and nano scale pores). Through the large number of solid/air interfaces created by such pores, it can efficiently tune the impedance matching. The solid/air interface renders surplus EM wave attenuation capabilities by increasing the EM wave trajectory path via internal scattering within the pores. The 3D graphene architectures-based polymer composites show hitherto EMI shielding efficiency improvement at significantly low mass density and percolation threshold. However, most of the existing studies on 3D graphene-based composites rely on trial-and-error methods without comprehensively investigating the effect of the geometrical and microstructures aspects on the EMI shielding performance. Furthermore, the state-of-art literature does not (re)present an analytical/theoretical model that can be employed to optimize parameters appropriate for designing the absorption-dominated shielding material with diminished reflection. This review is intended to cover the latest progress and innovation around 3D graphene nanostructure-based polymer composites as EMI shielding materials. The EMI shielding properties of the composites, including graphene aerogels, foam and hybrid aerogel/foam, with other dielectric and magnetic materials are discussed along with the underlying mechanism. In addition, this review represents an input impedance model that can be utilized in conjunction with experimental design to optimize geometrical and microstructural parameters to realize an absorption-dominated shielding material. Based on the available status on 3D graphene scaffold-based composites, we summarize the current achievements and offer a route toward future developments.
Among the conductive fillers mentioned above, the lowest electrical percolation threshold has been achieved with graphene, which is attributed to its high specific surface area, tunable electrical properties, and potentially connecting sheets.21,22 Achieving the targeted EMI shielding value at a lower percolation threshold is a significant advantage, as it reduces costs and the density of the composite material. In this regard, graphene, on account of its outstanding structure and characteristics, has been widely pursued in developing EMI shielding polymer composites.22,23 Reduced graphene oxide (rGO), a derivative of graphene that is mainly employed in developing composites, is considered a promising candidate due to its controllable dielectric loss that stems from residual functional groups and defects, which promote dielectric loss through defect polarization and dipole relaxation.24 Furthermore, the functional groups on its surface are conducive to anchoring other dielectric and magnetic materials, efficiently increasing the EM loss ability of the material and enabling the tailoring of impedance matching as well. Integrating the graphene/derivative of graphene with the polymer renders the seminal EMI shielding effectiveness (EMI SE) through electric and conduction loss.25 The EMI shielding performance of composites incorporating conductive fillers, whether in film or solid material form, mostly relies on conductivity. The high electrical conductivity of the filler network can cause an impedance mismatch between the shield and the air, enhancing the reflection and giving rise to secondary pollution.26–28 To circumvent secondary pollution, absorption-dominated materials are gaining attention as an EMI shield, where the EM wave absorption/reflection (A/R) ratio is expected to be greater than 1.29,30 A larger A/R ratio corresponds to less reflection, where the majority of incident waves are attenuated by the material through dielectric or magnetic loss. The integration of a microcellular 3D scaffold (foam, aerogel, sponge) with the polymer matrix has been considered a promising way to tailor the impedance matching and diminish the EM wave reflectivity.26,31 In this regard, the 3D graphene microcellular scaffold alone or its hybrid with magnetic, conductive, and other dielectric materials has been continuously pursued to enhance absorption through the interfacial and dipole polarisation loss mechanism.32,33 The 3D graphene-based architectures represent a highly interconnected micro/macroporous structure possessing ultra-low-density characteristics, and a high surface area with advantages of efficient flow of charge and ion.34 The 3D network in aerogels and foams reduces the buildup of conductive particles in the cell wall and yields an appropriate pore structure. Within this structure, trapped air optimizes impedance matching, thereby reducing reflection and enhancing absorption.35,36 Moreover, the structure of aerogels and foams contains multiscale pores (micro and nano-scale pores). Through the large number of solid/air interfaces created by these pores, they efficiently tune impedance matching. This interface provides surplus EM wave attenuation capabilities by increasing the EM wave path through internal scattering within the pores.6 Furthermore, the design of a 3D scaffold can assist with the uniform dispersion of filler, enabling the formation of a connected electrical network for efficient electron flow, thereby achieving superior shielding performance at lower filler loading. When it comes to nanofillers, regardless of their types, preventing their inevitable agglomeration within the polymer matrix is crucial to realizing their true potential.
To date, numerous studies on 3D graphene-based polymer composites have been reported, showing encouraging shielding effectiveness based on absorption-dominated mechanisms. However, there is a lack of studies focused on deciphering the significance of structural and geometrical factors in developing absorption-dominated shielding materials.32,37,38 For example, the scaffold thickness (geometry) and morphology (microstructure) can be a crucial variable affecting the surface impedance matching and reflectivity, the optimization of which can lead to high performance absorption-dominated shielding materials.39,40 However, most of the current studies have been executed on trial-and-error methods, hardly exploring the actual shielding mechanism governing the structure-EMI shielding performance of these class of materials. Studying the relationship between the thickness of the 3D scaffold, pore structure and corresponding shielding performance is crucial to obtaining an optimized reflectivity and A/R ratio critical for the absorption-dominant shielding material. In addition, there is a lack of analytical formulation-based approaches to provide direction and guidelines for modulating the structural design of absorption-dominated EMI shielding in 3D graphene architecture-based polymer composites, aiming to reduce reflection and achieve a high A/R ratio. Comprehensive review articles emphasizing analytical approaches that could save researchers’ resources and time in designing high-performance shielding materials are not readily available. Also, analytical formulation is crucial to understanding the underlying mechanism central to the structure-shielding properties. The effect of structural and geometrical factors on the optimal reflectivity and A/R ratio must be quantitatively studied to design an EMI shielding material with optimized absorption-dominant performance. This review article intends to cover the recent development of 3D graphene-based microstructure (GA and GF, along with hybrid multi-phase heterostructure) polymer composites in the realm of EMI shielding application, and represents an analytical approach that could be useful to optimize the geometrical and structural factors that are decisive toward achieving absorption-dominated 3D graphene-based polymer composites with reduced reflectivity. The represented input impedance model can be used to quantitatively assess the thickness dependence of the EM wave reflectivity, and provide guidelines for designing monolayer and gradient-layered structures consisting of 3D graphene and polymer with tailored impedance suitable for realizing an absorption-dominant mechanism. Fig. 1 schematically represents the EM radiation propagation and scattering across 3D graphene scaffold-based polymer composites. The current state-of-the-art, accomplished milestones, challenges, and future directions in this area have been discussed thoroughly.
Fig. 1 Schematic showing a propagation of the EM radiation, scattering and absorption in a 3D graphene-scaffold. |
(1) |
(2) |
In the above equation, ŷ and ẑ denote the admittivity and impedivity of the medium, respectively. μ is the permeability of the material, which can be written as μ = μ0μr. μ0 is the absolute permeability of air (1.268 × 10−6 H m−1), and μr is the relative complex permeability (material to air, μr = μ′ − jμ′′). σ is the conductivity of the material. ε is the permittivity of the material, and can be represented as ε = ε0εr. ε0 is the absolute permittivity of the air (8.85 × 10−12 F m−1), and εr is the relative complex permittivity (εr = ε‘ − jε′′). ω is angular frequency and can be written as ω = 2πf. Based on the wave eqn (1) and (2), the variations of the electric field along the thickness direction of the medium can be depicted by the propagation constant :40,42
E = Eie−γt | (3) |
(4) |
Here, α is the attenuation constant and β is the phase constant. The attenuation constant, α, can be written as function of ω, μ, σ and ε of the shield based on eqn (5).
(5) |
All homogenous materials are described by the intrinsic impedance, which is the ratio of E to H as represented in eqn (6), and transmission line theory requires the continuity of the input and output intrinsic impedance of the two media, or a reflection of the EM will occur.42
(6) |
For a dielectric material, σ ≪ ωε; hence, the impedance from eqn (6) can be written as:
(6a) |
For a conducting material, σ ≫ ωε; thus, the impedance from eqn (6) can be written as:
(6b) |
The impedance of an EM wave is defined by the tangential component of the electric field, E, and magnetic field, H, . For a homogenous layer of thickness t, the impedance can be expressed as below:39,43,44
(7) |
In the above equation, Z(t) is the impedance at interface t. Notably, a reflection will occur if Z(t) ≠ η.
The total shielding effectiveness (SE) is defined by:
SE = −20log10|T| | (8) |
The total shielding effectiveness comprises the absorption αA = 20log10|e−γt|, the reflection αR = 20log10|p|, and the successive internal reflection αB = 20log10|1 − qe−2γt|, where p and q are the transmission and reflection coefficients, respectively, and the value of T is written as;
T = p(1 − qe−2γt)−1e−γt |
Based on transmission line theory,45–47 the interaction between a propagating EM wave and EMI shielding material can be thought of as a circuit in the transmission line. Thus, layered materials with i numbers of layers can be modelled as multiple impedance components connected in series. A multilayer EMI shielding material with i layers can be considered to have i + 1 impedance sections in series in the circuit. Here, air serves as a substrate and hence considered as one impedance section in the circuit. In this situation, the perforating EM wave will undergo a reflection at each interface between all bordering impedance components. Therefore, the total reflectance (R) corresponding to the layered shielding material can be represented by a function of the output impedance (zout) and input impedance (zin):39,48,49
(9) |
As it is discussed, the reflection not only happens at the surface of the shield, but it also will occur between all adjoining sections with different impedances in the circuit. Thus, the surface input impedance for an EMI shield can be expressed as a function of the intrinsic impedance of the layer in consideration (ηi), propagation constant, γi, thickness (ti) of the layer in consideration (ith layer, surface layer), and the input impedance of subsequent sections (zi−1, surface impedance of the i – 1st layer), which can be represented as:39,43,44
(10) |
Then, the absorption of the i layers is written as:
αA = 20log10|eγ0t0 + γ1t1 + …γiti| | (11) |
The total reflection can be depicted as the sum of the reflection at each boundary (interface),
(12) |
αB = 20log10|(1 − q0e−2γ0t0)(1 − q1e−2γ1t1)…(1 − qie−2γiti)| | (13) |
As can be seen in eqn (11), the absorption is related to the propagation constant γi to σiμi as eqn (4), and to the film thickness, ti. According to eqn (12), the reflection does not depend on the thickness. However, it is characterized by the impedance ratio of the bordering layers. The internal re-reflection, akin to absorption, is also a function of the layer thickness. The impact of the reflection to the shielding effectiveness becomes more significant as the number of layers increases. The reflection mechanism at the interface between the two layers becomes critical and governs the shielding effectiveness. As absorption-dominated materials are becoming crucial to circumvent the effect of secondary pollution, theoretical models to guide the design and fabrication of optimal EM wave reflection shielding materials are paramount to address this issue. An input impedance model can be employed to reveal the effect of the microstructure (e.g., void fraction, pore size, cellular morphology) and structural (thickness) factor of each layer on the impedance matching and reflectivity of the layered foam/aerogel composites. This analytical model can guide the optimization of the structural and microstructural parameters of each layer to realize suitable input impedance matching and achieve an absorption-dominated shielding mechanism with reduced reflection.
The intrinsic impedance of the ith layer can be written as
(14) |
(15) |
It should be noted that, in most studies associated with semi-conductive materials, the σ term is neglected from the impedance equation as σ ≪ ωε. However, such practice in the case of conductive polymer composites with an electrical conductivity of more than 1 S m−1 may lead to an error that cannot be ignored. For 3D graphene (aerogel, hydrogel) polymer composites, two impedance components (composites and air substrate) must be considered in a circuit. Using eqn (7, 10, 14) and (15), the input impedance for a monolayer polymer composite shielding material can be represented as:
(16) |
As mentioned above, in EMI shielding materials, air serves as a substrate; hence, Zout = Z0 = 1. The R value of the material can then be defined as
(17) |
As per eqn (14) and (16), if the relative complex permeability, thickness, conductivity, and relative complex permittivity are known, the dependence of the reflectivity R on the thickness of each layer can be calculated, and this method is termed as the input impedance based on transmission line theory. This method can be employed to design multilayered shielding materials based on 3D graphene-based polymer composites with diminished reflectivity. The equations indicate that the scaffold thickness plays a crucial role in tuning the surface impedance matching conditions, and in realizing the diminished reflection for absorption-dominated EMI shielding. Furthermore, eqn (14)–(16) can be utilized to calculate the reflectivity of composites containing a 3D scaffold with varying cell sizes (pore sizes), volume fractions, and other parameters. The electrical properties and impedance characteristics of the 3D scaffold can be essentially adjusted by changing the pore sizes and volume fractions, which, in turn, can either increase or decrease the secondary reflection. The effective EM wave absorption ability of the 3D scaffold generally depends on their conductive network optimization and bulk density adjustment.50 The density of the scaffold can be altered by changing the pore size, while keeping the volume fraction constant. A scaffold with small pore sizes forms discontinuous cell walls, leading to fewer electrically conductive pathways. Conversely, a scaffold with large pore sizes forms an interconnected network, resulting in numerous conductive paths. Furthermore, the number of contact junctions in large pore size scaffolds is comparatively small, resulting in a diminished contact resistance due to the effective overlapping region. Wan et al. prepared graphene aerogels with different pore sizes, and observed that the scaffold with larger pore sizes exhibited higher electrical conductivity.51 This was attributed to a seamless interconnected network that enabled effective and rapid channels for electron transport, in contrast to the scaffold with smaller pore sizes. The decrease in electrical conductivity is beneficial for surface impedance matching, which in turn results in a reduced reflection of the EM waves. The EMI shielding performance of epoxy composites developed with the large pore size graphene aerogel was found to be higher than that of composites containing a small pore size scaffold. It should be noted that a decrease in the electrical conductivity often leads to a reduction in the EMI shielding efficiency, as the attenuation constant (eqn (5)) and permittivity are directly linked to the electrical conductivity. However, a recent study has shown that the absorption capability via dielectric loss in small pore size scaffolds compensates for the reduction in the electrical conductivity.39 Therefore, the model presented above can also be used to design scaffolds with optimum density and microstructure that attenuate maximum EM waves and reflect minimally.
Fig. 2 Preparation of the 3D graphene scaffold following different methods. (a) Fabrication of the free-standing GF through chemical vapor deposition (CVD) using Ni as the template, reproduced with permission from ref. 32, copyright reserved Elsevier 2020. (b) Preparation of the varied cellular structure GA employing GO precursors of different sizes by self-assembly, reproduced with permission from ref. 51, copyright reserved Royal Society of Chemistry 2016. (c) Fabrication of the rGO-GNF foam following the bubble template method, reproduced with permission from ref. 85, copyright reserved Elsevier 2021. (d) Schematic for the preparation of the Ag/GO foam by assembling and freeze-drying of the functionalized silver platelets and GO, reproduced with permission from ref. 92, copyright reserved Royal Society of Chemistry 2019. |
Fig. 3 Schematic depiction of the fabrication process of the anisotropic graphene/PDMS composite. (a) GO aerogels fabricated by bidirectional freeze casting technique. (b) GO aerogels with a lamellar structure formed after low temperature freezing dry at 10 Pa. (c) Graphene aerogels achieved by further thermal reduction of the GO aerogel. (d) Graphene/PDMS composites obtained by infiltrating PDMS into the graphene aerogel,and (e&f) GO aerogel before and after PDMS infiltration, reproduced with permission from ref. 37, copyright reserved Elsevier 2019. |
Fig. 4 Different fabrication processes of 3D graphene/polymer composites. (a) Schematic representation of the dip coating technique: (a1) graphene foam was dipped, (a2) held in the epoxy, and (a3) retracted from the epoxy resin, followed by room temperature curing, reproduced with permission from ref. 34, copyright reserved Elsevier 2018. (b) Schematic illustration of the fabrication process of GA/epoxy composites following the vacuum-assisted infiltration technique, reproduced with permission from ref. 68, copyright reserved American Chemical Society 2015. (c) Depiction of the fabrication of GNPs/rGO foam/epoxy composites by template method, reproduced with permission from ref. 83, copyright reserved Royal Society of Chemistry 2019. |
It is notable that only certain polymers (such as PDMS, epoxy) have been used to formulate a composite with the 3D graphene scaffold. This is likely due to the low viscosity of a polymer like PDMS, which facilitates its easy infiltration into the 3D scaffold. Also, the ease of processing and availability of those polymers with different viscosities provides the freedom to choose different fabrication techniques, such as coating, vacuum infiltration, 3D printing, etc. On account of their structural capabilities and good adhesion properties, epoxy and PDMS have been preferred polymers, which can be either coated or impregnated to develop 3D graphene scaffold composites. Furthermore, the presence of excellent surface chemistry between those polymers and the graphene scaffold enables the excellent wettability of the polymer onto the 3D structure.34 The low viscosity and improved wettability facilitate robust interfacial interactions between the polymer and 3D scaffold, which promotes the formation of a network, thereby increasing the electrical conductivity.
Fig. 5 Scanning electron microscopy micrographs showing the different microstructures. (a & b) Aerogels achieved from large size GO, and (c & d) obtained from small size GO; reproduced with permission from ref. 51, copyright reserved Royal Society of Chemistry 2016. |
In general, a high weight percentage of conductive fillers is required to construct a seamless electric network for composites with randomly oriented porous scaffolds. Therefore, to further lower the percolation threshold in porous structures, different strategies have been pursued to fabricate 3D conductive scaffolds with oriented structures.37 A 3D architecture with a highly oriented structure shows higher electrical conductivity at low filler content, thereby achieving high-performance shielding efficiency. To exploit the orientation-dependent EMI shielding properties, GAs with anisotropic microstructures have been used to fabricate composites for EMI shielding.70 Anisotropic GAs (AGAs) with highly aligned graphene networks were prepared by self-assembly of rGO, followed by directional freeze-drying method. Remarkably, the prepared AGAs scaffold showed different microstructures and performances along the axial (freezing direction) and radial (perpendicular to the axial direction) directions. Epoxy resin was impregnated within the AGAs scaffold assisted by vacuum. The highly aligned graphene/epoxy composite showed an EMI shielding effectiveness of 32 dB along the radial direction with 0.8 wt% thermally treated AGAs (TAGAs) coupled with the improved storage modulus. The shielding contribution from SEA along the radial direction was found to be higher than those along the axial direction. This is likely due to the hierarchical alignment of graphene sheets that increase the propagation path length of the EM wave. Due to the presence of numerous multifaceted surface areas rendered by GAs, the permeated wave suffers multiple reflection and scattering, resulting in the decay of radiation. The result reveals that confining the graphene nanosheets in the preferred direction could be more effective in designing a shielding material with absorption-dominated characteristics. A nacre-mimetic graphene network prepared by a unique bidirectional freezing technique incorporating polymer composites (with 0.42 wt% graphene) has revealed an EMI SE (∼65 dB) that is comparable to that of copper foil.37 The bidirectional freezing technique was adopted over unidirectional freezing to create a long-range aligned lamellar structure with tunable interlayer spacing and layer thickness. The prepared composites displayed anisotropic conductivities and mechanical properties, along with significant shielding performance, which was found to be dependent on the architecture of the 3D conductive network. The biaxially aligned lamellar structure creates many efficient interfaces within the composites, promoting multiple interlayer reflections that consume the electromagnetic radiation. The impact of the architecture of the conductive channel on SE, such as high layer density (more lamellar interfaces), was found to contribute more to absorption. The realization of such a high value of EMI SE at low filler loading indicates that to harness the optimum loss ability of the conductive filler, the meticulous design of a 3D scaffold is crucial for the development of high-performance EMI shielding polymer composites. Song et al. prepared rGO with a honeycomb structure (rGH) following freeze-drying & thermal annealing using an aluminium oxide (Al2O3) honeycomb as a template, which was then immersed into epoxy resins to fabricate rGH/epoxy composites that showed an EMI SE value of 38 dB.71 The improvement in SE was attributed to the multiple reflections within the honeycomb pores, and to the attenuation of the EM waves as it induces current inside rGH.
Chen et al. prepared porous GAs enhanced with phenolic resol resin by hydrothermal procedure, followed by annealing and incorporation into the epoxy resin to study the EMI shielding performance.72 It was believed that phenolic resol resin assisted the graphene sheets in coalescing into a hierarchical 3D macrostructure, assumed to be preserved during compounding with epoxy resin. The prepared AG induced high electrical conductivity within the epoxy resin, and the composites showed excellent EMI shielding performance. With the addition of only 0.33 wt% of the annealed aerogel, an electrical conductivity value of 73 S m−1 and an EMI shielding effectiveness value of 35 dB were recorded. The report systematically investigated the effects of thickness on the shielding performance, and it was found that as the sample thickness increased, the EMI shielding performance also increased. In another study, graphene-based aerogel film (AF)/PDMS composites have been prepared to explore the EMI SE of AF in a polymer matrix.73 The following infiltrating and curing single and multilayer rGO-AF/PDMS composites were prepared. The five-layer rGO-AF/PDMS composite with a density of 0.122 g cm−3 and a thickness of 1.547 mm exhibited an SE value of 53 dB at the X-band (8.2–12.4 GHz), and a specific SE of up to 434 dB cm3 g−1. The single-layer composite exhibited a reflection-dominated mechanism at lower frequencies, while absorption dominated at higher frequencies. Increasing the number of composite layers does not significantly impact the reflection efficiency. However, the absorption efficiency shows an increasing trend. The model presented earlier in this review article can be employed to understand how changing the thickness of the layer influences the EM absorption ability. The amount of secondary reflection can be minimized by adjusting the layer thickness of the material. Achieving strong loss ability and better impedance matching is crucial to realizing an absorption-dominated shielding mechanism. Heterogeneous interfaces originating from more than one component can elevate the loss abilities through synergistic effects, enhancing impedance matching and interfacial polarization loss, which are vital to achieving an absorption-dominated EMI shielding mechanism. Towards this, ternary mixtures of thermally annealed GA (TAGA), MWCNT and PANI have been designed to render epoxy composites with a synergistically robust triple conductive network.74 The PANI/MWCNT/TAGA/epoxy nanocomposites exhibited an EMI SE value of 42 dB and electrical conductivity of 52.1 S cm−1 at the mass ratio of 3:1 (GO to f-MWCNT) and the loading of 4.61 wt%. The promising results obtained from this study suggest that modulated and customized heterogenous interfaces can be generated by composition optimization, which would enhance the electromagnetic attenuation in the 3D graphene-based hybrid. There has been an upsurge in research activities on multifunctional composites, as current technologies expect a material to have more than one property and perform more than one function. A single attribute of a material is not enough if it is to be applied in a complex environment. Taking that into consideration, recent research studies are focused on designing composites with dual functionality or more. Recently, a 3D copper nanowires-thermally annealed graphene aerogel (CuNWs-TAGA) framework that was prepared by freeze-drying, followed by thermal annealing, was reported.75 Epoxy resin was poured into the prepared framework to achieve CuNWs-TAGA/epoxy composites for high thermal conductivity and EMI shielding effectiveness. It is worth noting that the composites revealed a thermal conductivity coefficient (λ) value of 0.51 W m−1 K−1, EMI SE value of 47 dB, and electrical conductivity (σ) of 120.8 S m−1. It is likely that the compounding of CuNWs and GA resulted in an abundant heterogeneous interface that was conducive to enhancing loss efficiency. It can be concluded that if the selection of the material is made prudently, it is possible to induce abundant heterogeneous interfaces, thereby enhancing the EM wave attenuation.
The colossal, interconnected network formed by the nodes and branches of graphene foam within the polymer matrix creates seamless channels for the rapid transfer of electrons. However, care must be taken to develop high-quality GF as the inter-sheet junction contact resistance lowers the electrical conductivity of GF. In an endeavour to improve the quality of the foam or decrease the inter-sheet junction contact resistance, the template-directed CVD method has been reported to design graphene/poly(dimethyl siloxane) (PDMS) foam composites.6 The amount of graphene and the electrical conductivity of the composites were tuned by varying the flow rate of methane during the CVD growth of graphene. The prepared composites exhibited a density of ∼0.06 g cm3, which is 20 times less than that of a solid polymer composite. With the loading of <0.8 wt%, an EMI SE as high as 30 dB was recorded with a specific EMI SE of up to 500 dB cm3g−1. Furthermore, the foam composites showed excellent flexibility, and their SE remained unaltered after repeatedly bending to a radius of ∼2.5 mm for 10000 times. The demand for lightweight electrical components crucial in applications such as next-generation aircraft and wearable devices has elevated the relevance of flexible polymer composites more than ever before. In this regard, continuous attempts have been made to develop flexible composites with superior EMI shielding efficiency, along with other attributes such as lower density and flexibility. Towards this, PDMS was directly infiltrated into a 3D interconnected graphene network using the vacuum-assisted technique.76
The super flexible composites showed an excellent electrical conductivity value of 103 S m−1 and EMI SE of around 54 dB with 3.07 wt% of graphene. A majority of the EM wave was absorbed by the composite, which made a significant contribution to the overall shielding mechanism. It was assumed that the 3D interconnected scaffold formed numerous multifaceted cells, promoting multiple reflections, and scattering that made the escape of the microwaves difficult. The presence of residual polar functional groups, defects, and multiple interfaces contributes to dipole polarization loss, thereby contributing to the overall loss mechanism. The development of a highly porous, bendable laterally compressed GF (cGF)/acrylonitrile butadiene styrene (ABS) composite with seminal shielding and certain strength has been reported to confer structural stability and superior shielding.32 The composite was prepared by dip coating ABS on a dense cellular anatomy of freestanding cGFs, which was achieved by growing graphene on laterally compressed Ni foam substrates. Isotropic cellular graphene foams were achieved, with similar openings between the skeletons along both the compression direction and perpendicular to it. The cellular foam retained its structure even after ABS was drop coated. It is worth noting that the composites showed a porosity of 89% and ultra-low density of 0.12 g cm−3. The 75%-cGF/ABS composites exhibited a distinctive two-layer structure comprising the cellular porous structure with ABS evenly coated on the graphene networks. The cGF/ABS system with a graphene content of 8 wt% delivered an electrical conductivity value of 635 S cm−1 and SE of 42.4 dB (at 50% compression), along with robust and bendable performances. These cGF/ABS composites display superior mechanical properties over other flexible polymer systems, such as GF/PDMS composites of comparable density.76 The absorption-dominant EMI shielding was ascribed to the efficient dissipation of surface currents by the high-quality meticulously designed graphene skeleton and quick thermal losses. Moreover, the laterally compressed GFs rendered denser graphene structures, leading to denser conductive networks per unit volume. The shielding performance of the composites decreases with the further rise in lateral compression degree (above 50%), which is indicative of annihilation of the conductive network at a higher degree of compression. This study reveals interesting findings that the electromagnetic absorption performance of the composites can be modulated by regulating the compression strain during scaffold growth. Ba et al. created a 3D network of graphene (TPU/G) by employing sodium chloride (NaCl) as the template and thermoplastic polyurethane (TPU) as the binder, which was subsequently carbonized to generate the C/G network, and encapsulated in epoxy resin.77 At 1.59 wt% of graphene loading, the SE value reached ∼38.78 dB. Meanwhile, at 7.60 wt% of graphene, the thermal conductivity value reached 1.19 W m−1 K−1. It is interesting to note that with the increase in the graphene content, the absorption coefficient values diminished, which is likely due to enhanced reflection with the accumulation of graphene sheets. In another report, microporous ultrathin graphene nanosheet foams have been reported by a salt-template-driven freeze-drying-calcination route with PEG 20000 and NaCl as a carbon source and a template, respectively.78 The calcination temperature (T) and PEG 20000/NaCl mass ratio (λ) were unutilized to modulate the texture, defects, graphitization, EMI SE, and thermal conductivity of the graphene foams. The graphene foams were created under T = 800 °C and λ = 0.530, and subsequently compounded with silicone rubber, exhibiting the optimal EMI SE and thermal conductivity, viz., 3.95 W (m K)−1 and EMI SE > 20 dB, respectively. The enhancement in SE was ascribed to the conductive loss (ε′′c), polarization loss (ε′′p), and multiple scattering that arose due to the strong shape anisotropy of the ultrathin graphene nanosheet foams, large specific surface area, high defects, small thickness, and porous 3D crosslinked frameworks. Conducting 3D networks at lower mass concentration of filler have been prepared by modifying GF using p-phenylenediamine (PPD), which anchors the reactive sites on GF for further in situ polymerization of PANI, leading to the formation of the network structure of GF/PANI.79 It is speculated that PANI promoted the connection of graphene sheets in GF, enabling the formation of the connecting network. After being compounded with epoxy, GF/PANI exhibited an EMI SE value of 38.32 dB. A novel leaf-like structure foam composed of CNTs and rGO (abbreviated as CGF) had been reported to reduce the density of the 3D structure, which was subsequently compounded with PDMS for EMI shielding applications.35 The presence of CNTs enabled the expansion of the conductive network and increased the electrical conductivity by 274.4%. The CNTs were firmly embedded into the graphene hole via π–π interactions. The leaf-like structure foam material exhibited a SE value of 71.4 dB. When compounded with PDMS, the composites retained 71.6% (71.1 dB to 50.9 dB) of SE after pressing 100 times under a pressure of 500 kPa. In another study from the same research group, a leaf-like 3D CNTs/GA film (CGAF) was designed, where CNTs were impeccably embedded in graphene, akin to the veins and mesophyll of a leaf.38 The prepared 3D CGAF scaffold exhibited an EMI SE value of 26.6 dB, which predominantly arose from the absorption of the EM wave rather than reflection. On compounding the CGAF scaffold with PDMS, an EMI SE value of 74.7 dB was reported, which corroborated the efficient flow of charges in the conducting network formed by seamlessly embedded CNTs and consumption of EM waves due to the multiple reflections in the 3D structure.
Drop coating of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS) on 3D freestanding GFs has been performed to fabricate GF/PEDOT:PSS composites for EMI shielding applications.80 The GF/PEDOT:PSS composites exhibited an ultralow density of 18.2 × 10−3 g cm−3 and a porosity of 98.8%, as well as an electrical conductivity value of 4320 S m−1. The so-formed highly conducting network and porous macro-structure assisted in the smooth transport of electric charge, which resulted in an SE value of 91.9 dB. The increased dielectric loss promoted the decay of the penetrating radiation, which led to a high absorption of EM waves. Dielectric loss of the composite is basically ruled by three electronic processes, viz., electronic displacement, space charge and interfacial polarization.81,82 It is likely that the network channel generated by the 3D macrostructure rendered a pathway for electromagnetic field-induced currents, resulting in the rapid decay of radiation. Fig. 6a shows the preparation of the free-standing graphene scaffold and composites, and the morphologies of the foam before and after coating (Fig. 6c and d), where a uniform coating of PEDOT:PSS can be seen on the 4-dodecylbenzene acid (DBSA)-functionalized graphene foam (Fig. 6d). The decrease in contact angle (Fig. 6e) with the increase in the concentration of DBSA indicates enhanced interactions of PEDOT:PSS with the graphene foam (Table 1).
Fig. 6 (a) Schematic procedure of the preparation of the GF/PEDOT:PSS composites; (b and c) SEM and TEM images of GFs before and (d) after PEDOT:PSS coating and (e) contact angles of the compressed GF plates as a function of the DBSA concentration. The inset in (c) is the TEM image of pristine graphene. The insets in (e) show the SEM images of the GF/PEDOT:PSS composites treated with different DBSA concentrations and the shapes of the corresponding PEDOT:PSS droplets (1, no treatment; 2, treated with 0.1 wt% DBSA; and 3, treated with 0.75 wt% DBSA), reproduced with permission from ref. 80, copyright reserved American Chemical Society 2017. |
Materials | Loading % | Preparation method | σ, S m−1 | EMI SE (dB) | Ref. |
---|---|---|---|---|---|
GA/epoxy | 1.0 | Infiltration technique | — | 30 | 51 |
Anisotropic GA/epoxy | 0.8 | Vacuum infiltration | — | 32 | 70 |
GA/phenolic resin | 0.33 | Vacuum infiltration | 73 | 35 | 72 |
Aerogel film/PDMS | Vacuum infiltration | 53 | 73 | ||
GA/PDMS | 0.42 | Self-assembly | 0.5 | 65 | 37 |
GA/MWCNT/PANI/epoxy | 4.61 | Template-casting method | 52.1 | 42 | 74 |
CuNW/GA/epoxy | — | Back filling | 120.8 | 47 | 75 |
rGO honeycomb/epoxy | 1.2 | Back filling | 40.2 | 38 | 71 |
GF/PDMS | 0.8 | Dip coating | 30 | 6 | |
GF/PDMS | 3.07 | Vacuum infiltration | 103 | 54 | 76 |
GF/ABS rubber | 8 | Dip coating | 635 | 42.4 | 32 |
Porous graphene/epoxy | 1.59 | Vacuum infiltration | 318.48 | 38.78 | 77 |
GF/Silicon rubber | 7 | — | 51.84 | >20 | 78 |
GF/PANI/epoxy | — | Dip coating | — | 38.32 | 79 |
CNTs/rGO foam/PDMS | — | Simple immersion | — | 71.1 | 35 |
GNPs/rGO foam/epoxy | rGO:GNPs 0.1:20.4 | Template method | 179.2 | 51 | 83 |
CNT/graphene aerogel/PDMS | — | Simple immersion | — | 74.7 | 38 |
GF/PEDOT:PSS | — | Drop coating | 4320 | 91.9 | 80 |
A facile bubble-template based strategy has been employed to create a 3D graphene network, wherein GO was employed to assist the assembly of GNP into a 3D porous framework structure.85 Vacuum-assisted infiltration of the liquid PDMS onto the as-prepared 3D skeleton was followed to fabricate the composites, which revealed a remarkable EMI SE of around 90 dB and a high thermal conductivity of above 3 W (m K)−1 with only 18.1 wt% of graphene content. Fig. 7a shows the optical microscope image of the foaming dispersion, wherein bubbles are seen to be uniformly distributed and closely packed together. Fig. 7b & c displays the digital images of the dried 3D rGO-GNP foam, which was able to endure a load that far heavier than its own. Fig. 7d–f depicts the microstructure of the as-developed 3D rGO-GNP foams with varying graphene contents. As discernible from the micrograph, the spherical holes left by the air bubbles are uniformly located in the foam scaffold. After careful observation, it is evident that as the graphene content increases, the extent of closure of each pore also increases. The 3D rGO-GNP-PDMS composites exhibited different contributions to the overall shielding with and without the annealing of 3D rGO-GNP. When using 3D rGO-GNP without annealing, both absorption and reflection contribute to the shielding, while annealing 3D rGO-GNP results in a more prominent contribution from reflection. It is assumed that annealing increases the electrical conductivity of 3D rGO-GNP by repairing damages on the graphene surface, rendering it a defect-free seamless conducting channel, which leads to the reflection of the EM wave. The 3D structures of the graphene nanoplatelets (GnP) and graphene fluoride (GF) have been fabricated in PDMS composites to study their EMI SE and thermal conductivity properties.86 The porous GnP@PDMS/GF composites showed an EMI SE value of 50.13 dB against 51.26 dB for only GnP@PDMS, which was attributed to the high conductivity of GnP and porous interconnected network responsible for the attenuation of the EM waves.
Fig. 7 (a) Optical microscopy image of the foaming emulsion, photographs of (b) the hydrogel and (c) the dried 3D rGO-GNP foam. Fracture surface SEM images of the 3D rGO-GNP foam with (d) 9.7 wt%, (e) 14.0 wt%, and (f) 18.1 wt% graphene content; reproduced with permission from ref. 85, copyright reserved Elsevier 2021. (g–i) Micrographs of the highly porous 3D TGCA3 aerogel and the fracture surface of the corresponding PTGCA3 composite (j–l) at different magnifications, where the SWCNTs nanostructures are firmly entangled with graphene; reproduced with permission from ref. 87, copyright reserved American Chemical Society 2018. |
In another study, a synergistic interconnected conductive network was generated by using pristine SWCNTs as secondary conductive fillers to prepare the rGO/SWCNTs aerogel.87 The PDMS/rGO/SWCNTs nanocomposite was developed by a facile backfilling approach to explore the EMI shielding properties. The compatibility of GO enabled SWCNTs to disperse uniformly within the polymer matrix, preserving the high conductivity of SWCNTs in the developed scaffold. The composites showed an electrical conductivity value of 120 S m−1 and an EMI SE of ∼31 dB over the X-band frequency range with an ultralow loading of 0.28 wt%. The unrivalled properties improvement ascertained the excellent synergy between rGO and SWCNTs in the aerogel system, contributing to significant dielectric loss. Fig. 7(j-l) shows the SEM images of the highly porous and interconnected 3D scaffold, where the entangled SWCNTs are wrapped into graphene sheets or act as efficient bridging to connect adjacent graphene layers. In another endeavour of a synergistic conductive network strategy, a highly porous GFs/CNTs/PDMS composite was fabricated.88 GFs were synthesized on a Ni substrate by CVD approach, and were mixed with the CNTs/PDMS suspension to fabricate the composites. The incorporation of CNTs in PDMS was found to significantly influence the charge transport property in the GAs/CNTs hybrid. The unique 3D hybrid composites with a porosity of 90.8% exhibited an EMI SE of 75 dB, an enhancement of 200% against 25 dB of the GFs/PDMS composites with the same graphene content and porosity. The significant improvement in the SE of the hybrid composites was attributed to the synergistic effect of GA and CNTs. While graphene aerogels absorb the EM wave by dissipating currents induced by electromagnetic fields, carbon nanotubes enhance the surface current dissipation by providing interconnected conductive networks and numerous interfaces for multiple reflections and polarization loss. The contribution of SEA towards the total SE was more prominent than that from SER, which is likely due to the extensive dissipation of surface currents. Employing the simple filtration and calcinations method, a 3D interconnected network was prepared using thermally treated graphene (G) and reduced oxidized multi-wall carbon nanotubes (r-OCNTs).89 A highly conducting flexible PDMS composite cake (TCGPC) was fabricated by coating PDMS onto the thermally treated r-OCNTs/G composite. The composite cake showed an electrical conductivity value of 15.15 S cm−1, which was attributed to the synergistic contribution of G and r-OCNTs. The EMI SE value was found to increase from ∼50.3 dB for G/PDMS to ∼67.3 dB for the composite cake in the X-band. It is important to note that the composite cake exhibited a stable EMI SE value with only 6.8% decrease after bending for 10000 times, which suggested that it was still able to block 99.99995% of the radiation. The remarkable improvement in the average SE was ascribed to the synergy in the conductive network provided by CNTs, as well as the enhanced electrical conductivity induced by calcinations. The composite cakes showed an absorption-dominated mechanism, which indicated that most of the EM decays into thermal energy via dielectric loss and interfacial polarisation loss. The energy consumption activity is accounted to the relaxation loss through interfacial polarisation and surface charge. Using the 3D graphene/MWCNTs foam as an electrically conductive skeleton, PDMS composites were fabricated for EMI shielding applications.90 The structure and composition evolution of the prepared foams were studied during the carbonization process from 1200 to 1600 °C and the graphitization at ultra-high temperature (2800 °C). It is considered that with the annihilation of polar functional groups, the repair of defects augments the ohmic loss while the polarization loss is reduced. An SE value of 54.43 dB at 1400 °C was reported. MWCNTs basically performed the three functions. First, it acts as a bridge to connect the gap between the 2D graphene sheets, rendering efficient electronic channels to the structure. Second, it functions as an impediment to the agglomeration of graphene sheets. Lastly, some MWCNTs extend to the outer edge of the graphene sheets, and act as electron polarization centres. The likely mechanism for such an improvement in SE was attributed to ohmic loss and polarization loss (electronic, dipole polarization), which is depicted in the interaction model diagram (Fig. 8a and b). Through this loss mechanism, the EM wave is mostly converted into heat and dissipated. In this study, the heat dissipation (measured as increased in temperature) was studied using infrared thermography, which is depicted in Fig. 8d. As indicated by the higher temperature, the thermal transfer rate in the composites seems superior to that of neat PDMS. As depicted in Fig. 8c, the developed composites show enhanced compressive strength, and the strength increases with the annealing temperature.
Fig. 8 (a and b) Schematic diagram of the EM shielding mechanism of the GC/PDMS composites. (c) Compression stress–strain curves of GC1400/PDMS and neat PDMS. The inset shows the optical images of GC1400/PDMS and the bent GC1400/PDMS. (d) Infrared thermography images of GC1400/PDMS and neat PDMS in heating for 10 s and 20 s (the hot stage with a temperature of 150 °C); reproduced with permission from ref. 90, copyright reserved Elsevier 2020. |
The design of a secondary conductive network conducive for EMI shielding using 3D graphene has emerged to assist in the dispersion of the conductive filler.91 A 3D silver platelets/rGO foam (AgPs/rGF) with numerous regular spherical hollow structures has been reported, wherein AgPs are uniformly dispersed along the rGO network assisted by 3D graphene.92 The interconnected 3D rGO channel resolved the agglomeration propensity of AgPs, and was eventually assembled with the secondary conductive network. Epoxy nanocomposites were prepared by backfilling the epoxy system on the 3D AgPs/rGF scaffold, which exhibited an electrical conductivity value of 45.3 S m−1 and SE 58 dB in the X-band with 0.44 vol% rGF and 0.94 vol% AgPs. The incorporation of AgPs shifted the shielding mechanism from an equal contribution of reflection and adsorption to being reflection-dominant. The study also validates the shielding ability of the 3D AgPs/rGF/EP nanocomposites to defy EM radiation by employing a finite element model to simulate the radiation process of the EM waves generated by the communication antenna to the brain, which is depicted in Fig. 9. A 12 V antenna was used for radiating EM waves to exposed and protected brain (protected by 3D AgPs/rGF/EP nanocomposites). Fig. 9d–d′′ depicts the map of the electric field distribution in the brain protected by 3D AgPs/rGF/EP, where the intensity of the radiated electric field is considerably reduced in air and the brain is seen to be almost unaffected. A study on Ag nanoparticle-decorated 3D porous rGO/polybenzoxazine composites also revealed enhancement in SE due to multi-reflections and current-induced magnetic dipoles.93 The magnetic losses-enhanced absorption mechanism led to an EMI SE value of 54 dB for the mentioned composites.
Fig. 9 Brain simulation exposed to electromagnetic radiation from the communication antenna. (a) Schematic diagram of the model prototype; (b) simplified radiation model. Model A: directly exposed brain to the electromagnetic radiation. Model B: protected brain to the electromagnetic radiation by 3D AgPs/rGF/EP nanocomposites; (c–c′′) map of the electric field distribution in the brain; (d–d′′) map of the electric field distribution in the brain under the protection of the 3D AgPs/rGF/EP nanocomposites. Reproduced with permission from ref. 92, copyright reserved Royal Society of Chemistry 2019. |
Aqueous GOs dispersants and one-dimensional (1D) silver nanowires (AgNWs) have been chosen to construct 3D rGOs/AgNWs bi-continuous conductive skeletons (GACSs).94 To minimize the high inter-sheet contact resistance and impede the agglomeration of rGO nanosheets, AgNWs were selected as a secondary building block to construct a 3D conductive scaffold. A modified sol–gel technique was applied to develop the GOs/AgNWs scaffold, which increased the pore sizes, pore-wall thickness, and structural homogeneity of the resulting composite scaffold. The scaffold was used to fabricate polydimethylsiloxane composites (PGACs) and the electrical, EMI shielding, and other properties were investigated. A series of PGACs were prepared, keeping constant the rGOs loading of 0.43% and varying the AgNWs loading, and they are represented as PG5A1C-0.53%, PG3A1C-0.6%, PG2A1C-0.66%, and PG3A2C-0.76%, respectively. The EMI SE of PGACs in the X-band was found to increase with the increase of the AgNWs amount, and reached the highest EMI SE of 34.1 dB at 0.43 wt% rGOs and 0.33 wt% AgNWs loadings. A significant enhancement in EMI SE was assigned to the synergy in conductivity between rGOs and AgNWs. Fig. 10 shows the variations of electrical conductivity, SET and the corresponding contribution from SEA and SER. According to Fig. 10b–d, the significant contribution to the total shielding was from the absorption-induced shielding. Conversely, the reflection is minimal, attributed to effective attenuation of the EM wave promoted by the 3D scaffold. With the higher electrical conductivity and improved impedance matching, the rapid localized current generations and faster thermal loss contribute to the total shielding.
Fig. 10 (a) Electrical conductivity and (b) SET of PDMS, PGC-0.43% and PGACs in the X-band, (c) SER, (d) SEA, (e) the average SET, SER, SEA, and (f) the average power coefficients (A, R, T) of PGC-0.43% and PGACs in the X-band; reproduced with permission from ref. 94, copyright reserved Elsevier 2019. |
Mimicking natural porous materials, a bio-inspired approach based on polydopamine interface buffer for the preparation of a carbon nanowires/graphene (CNWs/G) sponge composite has recently been reported.95 CNWs were uniformly grown on the graphene structure through covalent C–C bonding. A multi-scale structure was designed to maximize the absorption mechanism, where porous graphene behaved as a sponge skeleton and provided high electric conductivity. The in situ grown CNWs served as flagella that rendered strong EM absorption competency. The junction between the CNWs with graphene and the defects present in CNWs led to strong polarization loss, and hence the attenuation of the permeating radiation. The CNWs/G/PDMS composite showed an EMI SE value of 36 dB in the X-band and the composite density was found to be 97.1 mg cm−3. The improvement in SE was attributed to the unique sponge macrostructure of graphene and CNWs with the covalent junction interface, which spawned a strong polarization loss and promoted multiple reflections of EM waves. A hybrid structure of the 3D scaffold has shown great potential in EMI shielding applications. However, achieving a mechanically robust 3D scaffold with a high SE value is still a daunting challenge. Towards this, Fan et al. reported the fabrication of a microcellular epoxy foam containing a hybrid reduced graphene oxide (rGO)/short carbon-fiber (SCF) aerogel following the “gelation-press drying-impregnation & micro-foaming” method.96 The air-drying method was employed to control the network structure of rGO/SCF, which resulted in a transformation of the isotropic honey-comb structure into an anisotropic multilayer corrugated structure. The purpose of SCF was to provide stability to the carbon network that would keep the porous structure intact. The anisotropic microcellular epoxy composites showed an EMI shielding value of 95.5 dB (Table 2).
Materials | Loading % | Preparation method | σ, S m−1 | EMI SE (dB) | Ref. |
---|---|---|---|---|---|
Edge-rich graphene/rGO/epoxy | 3.98 | Vacuum infiltration | 68.2 | 45.9 | 84 |
GO/GNP/PDMS | 18.1 | Vacuum infiltration | — | 90 | 85 |
GNP/graphene fluoride/PDMS | 30 | Molding | 0.6 | 50.1 | 86 |
rGO/SWCNTs/PDMS | 0.28 | Backfilling | 120 | 31 | 87 |
GFs/CNTs/PDMS | GF:CNT 2.7:2 | Simple deposition | 31.5 | 75 | 88 |
CNTs/graphene/PDMS | — | Vacuum infiltration | 15.15 | 67.3 | 89 |
3D graphene/MWCNTs/PDMS | 0.98 | Vacuum infiltration | 100.99 | 56 | 90 |
rGOs/AgPs/PDMS | rGOs:AgPs 0.33:0.43 | Backfilling | 45.3 | 58 | 92 |
Ag/rGO/polybenzoxazine | Ag:rGO 15:25 | — | 0.005 | 54 | 93 |
rGOs/AgNWs/PDMS | 0.76 | Backfilling | 0.108 | 34.1 | 94 |
CNWs/G/PDMS | Dip coating | 0.34 | 36 | 95 | |
rGO/short carbon-fiber/epoxy | — | Foaming | 2365.0 | 95.5 | 96 |
Based on the above equation, to achieve the desirable impedance matching performance, it is crucial to make μ relatively close to ε. In order to improve loss mechanism for better EMI shielding, recently two phase heterostructures consisting of magnetic nanoparticles and graphene have evoked wide attention.98–102 3D graphene-based scaffolds have tunable porosity, which offers points to anchor magnetic components. Magnetic metals (such Fe, Co, Ni or their oxides) have been used with graphene or with a combination of graphene and CNTs to fabricate a 3D integrated architecture. The large single architecture, created through strong synergy, enhances EMI SE by improving the eddy current loss, natural resonance, exchange resonance, and multiple scattering processes. In addition to that, the combination of magnetic materials with the dielectric foam/aerogel improves the permeability of the scaffold, thus achieving an ideal impedance match that is conducive to the absorption-dominated shielding mechanism. The magnetic loss contributed by the magnetic medium to the overall shielding mainly arises from the exchange resonance, natural ferromagnetic resonance and eddy current loss.103 Towards improving the impedance matching and EM loss through magnetic materials, numerous absorption-dominated graphene aerogels or foams-based composites recently have been developed. For example, the Fe3O4/thermally annealed graphene aerogel (Fe3O4/TAGA)/epoxy nanocomposites were fabricated to study the EMI SE.104 At first, ethylene diamine functionalized Fe3O4 (NH2–Fe3O4) nanoparticles and GO were compounded, followed by the addition of L-ascorbic acid, to obtain Fe3O4/TAGA by thermal annealing method. Fe3O4/TAGA exhibited a pore structure, which is considered advantageous for multiple-reflection and hence for the effective attenuation of EM radiation. The Fe3O4/TAGA/epoxy nanocomposites showed an electrical conductivity value of 27.5 S m−1 when the mass ratio of GO to NH2–Fe3O4 was 2:1 and the total mass fraction of Fe3O4/TAGA in the composites was 2.7 wt% (1.5/1.2 wt% Fe3O4/TAGA). The corresponding Fe3O4/TAGA/epoxy nanocomposites showed the highest EMI SE of 35 dB in the X-band. The significant improvement in SE was ascribed to the large conductive network formed, and the combination of dielectric and magnetic loss, leading to a superior impedance match. With the increase in the loading of NH2–Fe3O4, SEA was found to increase, suggesting that the addition of NH2–Fe3O4 proved beneficial for shielding improvement contributed by magnetic loss. Fig. 11 shows the schematic for the fabrication of the Fe3O4/TAGA/epoxy nanocomposites.
Fig. 11 The schematic for the fabrication of the Fe3O4/TAGA/epoxy nanocomposites; reproduced with permission from ref. 104, copyright reserved Elsevier 2019. |
Fe3O4@anisotropic reduced graphene oxide aerogel/epoxy (Fe3O4@AGA/EP) nanocomposites have been reported, where Fe3O4@AGA was prepared by hydrothermal reduction reaction, followed by unidirectional freezing approach.105 Due to the synergistic effect arising from the magnetic and dielectric loss properties, the EMI SE of the Fe3O4@AGA/EP nanocomposites attained 40.4 dB along the radial direction when the mass ratio of Fe3O4:GO was 2:1. In another study, to derive the synergistic response, a unique structure was proposed by anchoring magnetic Fe3O4 nanoparticles onto the conductive 3D GF, and flexible PDMS composites were subsequently prepared.106 The unique structure was realised by assembling CTAB-modified Fe3O4 and GF through mutual electrostatic interactions. The flexible composite has an advantage over the rigid one as it can be easily mounted on an irregular and curve structure. The EMI SE value of ∼32.4 dB for the Fe3O4/GF/PDMS composite (∼1.0 mm) was recorded in the frequency range of 8.2–12.4. The significant absorption contribution resulted from the synergy between GA, and the improved SE was attributed to the magnetic Fe3O4. Integration of 1D CNTs with 2D graphene to design a 3D continuous network has recently been performed to enrich the EMI SE.107 The seminal improvement in SE further encouraged researchers to anchor magnetic particles on the 3D-CNTs skeletons, and to comprehend how this reasonably designed multiple structure played a role in improving the SE. A single integrated multi-phase hetero-nanostructure consisting of graphene, CNT and Fe2O3 (3D G–CNT–Fe2O3) was synthesized to fabricate the PEDOT:PSS/3D G–CNT–Fe2O3 composites film for EMI shielding application.108 The 3D G–CNT–Fe2O3 nano-architecture was synthesized by a microwave irradiation method with ferrocene as an iron catalyst and carbon source for CNT growth on graphene. The flexible composite films were fabricated based on PEDOT:PSS, and various graphene-based fillers (such as 2D rGO, 2D G–Fe2O3, and 3D G–CNT–Fe2O3) were fabricated to ascertain the strong synergistic effect of 3D G–CNT–Fe2O3 on the EMI shielding properties of the films. The three-phase 3D G–CNT–Fe2O3 hetero-architecture showed improved reflection, absorption and scattering of EM radiation, which was ascribed to the strong synergy among 2D graphene, 1D CNT and 0D Fe2O3. The electrical conductivity values of PEDOT:PSS, 2DrGO/PEDOT:PSS, 2D G–Fe2O3/PEDOT:PSS, and 3D G–CNTFe2O3/PEDOT:PSS were found to be 15400, 16200, 17400, and 22800 S cm−1, respectively. The EMI SE of the 2D rGO/PEDOT:PSS, 2D G–Fe2O3/PEDOT:PSS, and 3D G–CNTFe2O3/PEDOT:PSS composites films were found to be enhanced by 8%, 19%, and 25%, respectively. The remarkable improvement in SE was attributed to the excellent electrical conductivity of the multi-layered and interconnected nano-architecture, which assisted the easy delocalization of electric charges within the PEDOT:PSS network. Furthermore, iron particles induced a higher hysteresis and larger energy dissipation within the film. It is noteworthy that all the composite films exhibited an absorption-dominant mechanism rather than reflection, suggesting a synergistic contribution of the magnetic loss and dielectric loss. Fe3O4-decorated CNTs/rGO foam/epoxy (3D Fe3O4–CNTs/rGF/EP) nanocomposites with highly oriented 3D structures were fabricated by a facile template method.109 The prepared composites with 0.24 wt% rGF and 2.76 wt% Fe3O4–CNTs resulted in a remarkable electrical conductivity of 15.3 S m−1 and EMI SE value of 36 dB within the X-band range. The synergistic response from the magnetic loss and efficient 3D framework structures was assumed as a reason behind such enhancement. The prominent interfacial contacts between CNTs, Fe3O4 and rGF resulted in an improved interfacial polarisation relaxation, leading to EM attenuation. From the absorption-dominant mechanism of the composites, it can be concurred that the introduction of Fe3O4 particles significantly promoted magnetic and dielectric losses. Amino-functionalized FeNi alloy particles (f-FeNi) have been loaded on the 3D GO regular honeycomb structure (GH) skeleton. This was followed by in situ reduction to prepare the rGH@FeNi aerogel, which was then impregnated by an epoxy resin following vacuum-assisted method to prepare the rGH@FeNi/epoxy composites for EMI shielding application.33 The so-designed honeycomb conductive/magnetic structure expands the transmission path of the EM waves, leading to the increased attenuation of the EM waves by multiple reflections and scattering. Furthermore, the enhanced impedance matching between the rGH 3D conductive skeleton and epoxy resin matrix leads to increased hysteresis loss of the electromagnetic waves in the composites, which resulted in an SE value of 46 dB (Tables 3).
Materials | Loading % | Preparation method | σ, S m−1 | EMI SE (dB) | Ref. |
---|---|---|---|---|---|
Fe3O4/GA/epoxy | Fe3O4:GA 1.5:1.2 | Template-casting | 27.5 | 35 | 104 |
Fe3O4@GA/epoxy | 2.1 | Vacuum infiltration | 32.1 | 40.4 | 105 |
Fe3O4/GF/PDMS | — | Dip coating | 0.25 | 32.4 | 106 |
3D G-CNT-Fe2O3/PEDOT:PSS | 0.28 | Solution casting | 228 | 130 | 108 |
Fe3O4-CNTs/rGF/epoxy | rGF:Fe3O4–CNTs 0.24:2.76 | Template | 15.3 | 36 | 109 |
rGO@FeNi/epoxy | 2.1 | Vacuum infiltration | 38.7 | 46 | 33 |
3D graphene-based/polymer composites | 2D graphene-based/polymer composites | ||||||||
---|---|---|---|---|---|---|---|---|---|
Material | Loading (%) | σ, S m−1 | EMI SE (dB) | Ref. | Material | Loading (%) | σ, S m−1 | EMI SE (dB) | Ref. |
GA/EP | 1 | — | 30 | 51 | Graphene/EP | 2.5 | — | 29 | 114 |
GA/PDMS | 0.42 | 0.5 | 65 | 37 | rGO/PU | 2.5 | — | 53 | 115 |
3D graphene/MWCNTs/PDMS | 0.98 | 100.99 | 56 | 90 | Graphene-MWCNT/PU | 10 | — | 47 | 116 |
Porous graphene/EP | 1.59 | 318.48 | 38.78 | 77 | rGO/PU | 3.17 | 2.77 | 21.8 | 117 |
rGOs/AgNWs/PDMS | 0.76 | 0.108 | 34.1 | 94 | Graphene/SiCnW/PVDF | 9.5 | 1.5 | 32.5 | 118 |
rGOs/AgPs/PDMS | 0.76 | 45.3 | 58 | 92 | GNP/Ni/PVDF | 13 | — | 55.8 | 119 |
GF/PDMS | 0.8 | 30 | 6 | Graphene/WPU | 5 | 43.6 | 38 | 120 | |
GF/PDMS | 3.07 | 103 | 54 | 76 | GNS/TPU | 0.12 (Vol) | 35 | 14 | 121 |
GF/Silicon rubber | 7 | 51.84 | >20 | 78 | rGO/PEI | 2.5 | — | 22–26 | 122 |
GA/phenolic resin | 0.33 | 73 | 35 | 72 | GNP/PEK | 5 (Vol) | 2 | 33 | 123 |
Based on the available information, it can be conferred that the 3D graphene architectures shall accelerate the prospect towards the fabrication of high-performance absorption-dominated shielding materials. Although it will be too early to expect the engagement of these materials in industrial realm, the recent research activities nonetheless point towards a bright beginning. The crucial future directions that need to be undertaken for EMI shielding materials are as follows.
1. The current methods for designing 3D graphene scaffolds require innovative processing technologies that offer flexibility in regulating the pore size, creating ordered structures with aligned cell walls, customizing the cellular morphology to the desired scaffold properties, and controlling the thickness to achieve absorption-dominated shielding materials. Towards this, 3D printing technology holds the potential not only in providing freedom on the nanofiller proportion and size, but also renders the opportunity to design a scaffold having hierarchical pores that are apt for EM absorption. There have been a few reports on 3D printed graphene-based EMI shielding materials. For instance, Guo et al. reported on the shielding effectiveness value of 8.75 dB for a 3D printed lamellar graphene aerogel. Furthermore, a 3D printed lamellar Ti3C2Tx MXene/graphene hybrid aerogel has been reported by Hua et al.110 However, the poor interlayer adhesion between the printed layers of the 3D printed scaffolds is an issue that needs to be studied with rigour. Furthermore, the development of polymer composites holding these 3D printed scaffolds requires more investigations to examine the feasibility of these structures.
2. An interesting strategy for fabricating 3D graphene-based aerogels and foams using the electrospinning technique has recently attracted much attention. These 3D structures, with their innovative architecture, have the potential to serve as EMI shields due to their creation of new interfaces and high porosity, which expand the paths for reflecting and scattering electromagnetic radiation. The known fabrication process includes precision electrospinning, self-assembly, multi-layer spinning, liquid/3D collectors, and processing into bulk aerogels and sponges.111 Especially, precision electrospinning could be a potential technique to fabricate a highly porous 3D structure as it combines the additive manufacturing technique to exactly deposit the nanofiber in a predesigned pattern. A 3D macrostructure with heterointerfaces and excellent porosity has been prepared by assembling electrospun nanofibers. This process can be extended to prepare a graphene-based 3D structure, as well as through advanced formulation and optimization. Zheng et al. reported on an interfused core–shell heterogeneous reduced rGO/MXene aerogel (GMA) via coaxial wet spinning and freeze-drying, which exhibited an SE value of 83.3 dB that is supposedly higher than most of the carbon-based aerogels and foams.112 Construction of Ti3C2Tx MXene@GO hybrid aerogel microspheres (M@GAMS) via electrostatic-spinning technique assisted by rapid freezing and freeze drying was also reported, and the study included the microwave absorption performance.113 The design of 3D graphene aerogels and foams via electrospinning invoked exciting prospects. However, the issues concerning the mechanical stability is a big impediment. Studies covering the mechanical robustness of such materials that are desirable for use in complex environments are scarce. Hence, it is premature to comment on the suitableness of such materials for EMI shielding applications. Furthermore, dispersing these 3D microscopic structures in a polymer matrix is another big challenge. As of now, not much progress has been made in this route.
3. The design of gradient-layered structures is a promising strategy to achieve low reflection and absorption-dominated EMI shielding. These structures consist of one or more absorption layers, which attenuates the EM radiation, and a reflection (shielding) layer, which reflects and attenuates the remaining EM radiation. The interface between the layers can produce substantial interfacial polarization that enhances attenuation via polarization loss. A few reports on a MXene-based layered composite foams EMI shielding material with an absorption-dominated mechanism are available. The strategy can be extended to 3D graphene-based polymer composites as well.
4. Considerable intervention in theoretical understanding is expected to build a consensus on the mechanism responsible for shielding, and to understand the modus operandi of different dimension particles, microstructural, and geometrical effects on the shielding performance. Therefore, more efforts in computational studies and analytical modeling are solicited to optimize the microstructural and geometrical aspects for achieving absorption-dominated shielding. Not only is a theoretical approach required to understand how the microstructures and geometry of the 3D skeleton enable the improvement in shielding effectiveness at a rudimentary level, but comprehending the interaction at the atomic level also could be relevant for devising suitable microstructure materials.
This journal is © The Royal Society of Chemistry 2024 |