The effect of adding Bi3+ on the performance of a newly developed iron–copper redox flow battery

Daniel Manaye Kabtamua, Guan-Yi Lina, Yu-Chung Changa, Hsueh-Yu Chena, Hsin-Chih Huanga, Ning-Yih Hsub, Yi-Sin Choub, Hwa-Jou Weib and Chen-Hao Wang*a
aDepartment of Materials Science and Engineering, National Taiwan University of Science and Technology, 10607, Taipei, Taiwan. E-mail: chwang@mail.ntust.edu.tw; Fax: +886-2-2737-6544; Tel: +886-2-2730-3715
bInstitute of Nuclear Energy Research, Atomic Energy Council, Executive Yuan, 32546, Taoyuan, Taiwan

Received 30th November 2017 , Accepted 10th February 2018

First published on 23rd February 2018


Abstract

In this paper, we propose a new, abundant, cost-effective, non-toxic, and environmentally benign iron–copper redox flow battery (Fe/Cu RFB), which employs Fe2+/Fe3+ and Cu+/Cu0 as the positive and negative electrolytes, respectively. The effect of graphite felt (GF) electrode modification and addition of Bi3+ into the electrolytes on the performance of the Fe/Cu RFB were investigated. It was found that the cell containing Bi3+ in the electrolytes revealed higher coulombic efficiency (89.18%) and energy efficiency (35.24%) than the cell without Bi3+ (CE = 84.10% and EE = 34.43%) at 20 mA cm−2. This is because after adding Bi3+, Cu metal precipitation was not observed on the electrode surface, which indicates that the deposition process was potentially reversible on the electrode material, thus leading to enhanced performance of the battery. Furthermore, the efficiencies of the battery are stable over 10 cycles, which demonstrates that Fe/Cu RFB exhibits good stability on the microwave heat treated GF plus one layer microwave heat treated carbon paper (HT-GF + HT-CP) electrode after adding Bi3+ into the electrolytes.


1. Introduction

Due to the environmental concerns over burning of fossil fuels and their limited resources, along with the rising energy demands for the increasing global population, the utilization of clean and renewable energy generated from renewable sources, such as wind and solar, have attracted considerable social and scientific attention in recent years. However, the varied nature of such intermittent sustainable energy sources makes it difficult to integrate this valuable energy into the electrical grid supply. Therefore, a large-scale electrical energy storage system is needed to alleviate this problem.1–4

Redox flow batteries (RFBs) are one of the most promising energy storage system technologies owing to their attractive features such as high efficiency, intrinsic safety, short response time, deep discharge ability, long cycle life, and tolerance to over-charge and over-discharge.2,3,5,6 In redox flow batteries, large amounts of energy are stored in a pair of reduced and oxidized electro-active species dissolved in two separate liquid electrolytes alleged outside of the cell-stack. This permits us to independently scale up the power and energy components of the system (up to multi-MW and multi-MW h, respectively) by maintaining all of the electro-active species in a fluid form.7–10 The decoupling of the energy storage and power generation supplies provides a substantial design opportunity to independently scale-up the power capability or energy capacity for various energy storage system applications.11

Among the numerous types of RFBs that have been reported to date,12,13 all-vanadium redox flow batteries (VRFBs), originally proposed by Skyllas-Kazacos et al.,14 are highly suitable and widely studied for large-scale energy storage systems because of the good electrochemical reversibility of vanadium redox couples. In addition, they use active species of the same vanadium metal as the electrolytes, which substantially minimizes the problem of active component crossover contamination across the membrane.15,16 However, the limited earth-abundance and high cost of vanadium and the relatively low energy efficiency of the VRFBs still hinder their widespread commercial adoption.6 A feasible strategy to reduce the cost of RFBs should therefore be considered in terms of materials, cell configurations, and fabrication processes. Therefore, developing alternative low-cost and low-toxicity electrolyte materials is critical in RFBs.1

The all-iron redox flow battery (Fe RFB) was first pioneered by Hruska and Savinell in 1981.17 It utilizes the Fe3+/Fe2+ and Fe2+/Fe redox couples in positive and negative electrolytes, respectively, and is suitable for grid-scale energy storage applications. This is because of the availability, low-cost, and environmentally benign status of the active element (Fe).18 However, there are challenges in achieving the successful commercialization of this redox flow battery, such as low coulombic efficiency, hydrogen evolution and poor deposition/dissolution kinetics at the negative electrode, high self-discharge rate, and poor cycle life.19

The iron–chromium redox flow battery (Fe/Cr RFB) is an attractive alternative to the traditional RFBs. The Fe/Cr RFB has been considered as the first true RFB and utilizes low-cost and completely soluble redox-active materials in both the positive and negative electrolytes.13 In the Fe/Cr RFB battery, the Fe2+/Fe3+ redox couple is used in the positive half-cell while the Cr2+/Cr3+ redox couple is used in the negative half-cell. The Fe2+/Fe3+ redox couple exhibits a high electrochemical reversibility on carbon and graphite felt electrodes at the positive side. However, a catalyst is required at the negative side due to the relatively slow kinetics of the Cr2+/Cr3+ couple on these electrodes. Moreover, hydrogen evolution occurs as a side reaction to the reduction of the Cr3+ species, which reduces the coulombic efficiency and causes capacity decay.20

Recently, all-copper redox flow batteries (Cu RFB) have attracted tremendous attention for practical applications because copper is highly abundant with high purity and also, it is inexpensive, less toxic, and highly soluble in water.21 Furthermore, the carbon electrodes and the polymeric separators that can be applied in the all-copper system are also relatively cheap materials and the heat exchangers are eliminated.21 RFBs based on the chemistry of copper employ the three oxidation states of copper, namely, Cu(s), Cu+ and Cu2+. Among these, the Cu+ ion is unstable and undergoes disproportionation to form Cu(s) and Cu2+ at ambient temperature and pressure. However, Cu+ can be stabilized by forming a complex with suitable complexing agents such as chloride ions. Previous studies have shown that Cu+ the complexes CuCl(aq) and/or CuCl2 are dominant in dilute acid chloride solutions, while high order chloro-complexes, for instance, CuCl32− and/or CuCl43− become more stable at higher concentrations of chloride ions.22 One of the main limitations of an all-copper redox flow battery is a relatively low cell voltage (0.6 V), which is considerably lower than those of other traditional RFBs (>1.15 V).23

In this study, by combining the numerous benefits of the iron and copper redox flow battery systems, we propose a new, abundant, cost-effective, non-toxic, and environmentally benign iron–copper redox flow battery (Fe/Cu RFB), which employs Fe2+/Fe3+ and Cu+/Cu0 as the positive and negative electrolytes, respectively, as shown schematically in Fig. 1. A standard cell voltage of 0.25 V was produced through the following electrochemical reactions in a Fe/Cu RFB:


image file: c7ra12926b-f1.tif
Fig. 1 Schematic illustration of the experimental set-up of a Fe/Cu redox flow battery.

Positive electrode:

 
Fe2+ ↔ Fe3+ + e, E0 = 0.77 V (1)

Negative electrode:

 
Cu+ + e ↔ Cu0, E0 = 0.52 V (2)

Cell reaction:

 
Fe2+ + Cu+ ↔ Fe3+ + Cu0, E0 = 0.25 V vs. SHE (3)

During the charging process, ferrous ions (Fe2+) are oxidized to ferric ions (Fe3+) in the positive half-cell, while cupreous ions (Cu+) are reduced to copper metal (Cu0) in the negative half-cell. When the battery is in the discharge process, reversed reactions take place. The effect of GF electrode modification and addition of Bi3+ to the electrolytes on the performance of the Fe/Cu RFB are investigated. It was found that the cell containing Bi3+ in the electrolytes revealed higher coulombic efficiency (CE = 89.18%) and energy efficiency (EE = 35.24%) than the cell without Bi3+ (CE = 84.10% and EE = 34.43%) at a current density of 20 mA cm−2. Furthermore, after adding Bi3+ into the electrolytes, the efficiencies of the battery are stable over 10 cycles, which demonstrates that Fe/Cu RFB has a good stability on the microwave heat treated graphite felt plus one layer microwave heat treated carbon paper (HT-GF + HT-CP) electrode under these conditions.

The main shortcoming of the Fe/Cu RFB is its relatively low cell voltage. The cell voltage is significantly lower than those of other RFB systems, leading in principle, to lower values of energy density. However, high solubility of iron and copper in aqueous solution (by increasing the concentration of active species used in the electrolyte) may overcome this issue in the future. The use of high amounts of iron and copper are not a key issue in terms of cost since these materials are abundant, less toxic, and cheaper than other redox pairs commonly used in these technologies. For example, compared with vanadium metal, the use of iron and copper are more attractive for broad market penetration as they have a lower cost ($2.4 kg−1 of iron and $7.4 kg−1 of copper versus $23.5 kg−1 of vanadium).20,23 The major conclusion drawn from our study is that a small cell voltage does not render the Fe/Cu RFBs ineffective to store energy efficiently. In addition, the low cell voltage clearly benefits the coulombic efficiency of the system with slight tendency for electrode side reactions to occur at a higher current densities.24

2. Experimental

2.1. Preparation of electrolytes

In this study, all reagents were used without further treatment. The iron electrolyte was prepared by dissolving 1.5 M of FeCl2 in 3 M HCl solution, while the copper electrolyte was prepared by dissolving 1.8 M of copper(I) chloride (CuCl) in mixed supporting electrolyte (CaCl2 + HCl). In order to increase the concentration of chloride in copper electrolyte solution, 2.4 M of CaCl2 and 2.4 M of HCl were utilized as a mixed supporting electrolyte. All solutions were prepared with distilled water at room temperature.

2.2. Electrochemical measurements

Cyclic voltammetry (CV) measurements were performed using a typical three-electrode cell at room temperature. A platinum wire and Ag/AgCl were used as the counter and reference electrodes, respectively. The working electrode was a glassy carbon (GC) disk with a geometric surface area of 0.196 cm2. For the iron half-cell, a CV test was performed in 1.5 M FeCl2 in a 3 M HCl solution in the potential range between −0.5 and 1.2 V versus Ag/AgCl, while for copper half-cell, a CV test was performed in 1.8 M CuCl in a mixed supporting electrolyte (2.4 M CaCl2 + 2.4 M HCl) in the potential range between −0.7 to 1.0 V versus Ag/AgCl. During the tests, various scan rates (10–70 mV s−1) were used. A CV test was also performed for both iron and copper half-cell electrolytes without and with 0.01 M Bi2O3 at a scan rate of 50 mV s−1. The electrolytes were nitrogen-purged to avoid undesired oxidation. All electrochemical measurements were performed using a potential station (Solartron 1280C).

2.3. Charge–discharge tests of Fe/Cu RFB

A Fe/Cu RFB single cell test was performed using a 25 cm2 (5 cm × 5 cm) area of the modified graphite felt (GF) electrodes for both the negative and positive sides. A modified GF electrode was prepared using microwave thermal treatment. A pristine GF and one layer carbon paper (CP) were heat treated at 400 °C for 15 min and then cooled to ambient temperature before use. The main objective of the heat treatment of pristine GF and CP was to improve their electrochemical activity and wettability. A pristine Nafion 117 membrane was used as a separator. The cell was connected to two glass reservoirs holding a balanced volume of electrolytes (50 mL) on both negative and positive sides. The concentration of electrolytes was 1.5 M FeCl2 in 3 M HCl solution and 1.8 M CuCl in a mixed supporting electrolyte (2.4 M CaCl2 + 2.4 M HCl) solution in the positive and negative sides, respectively. Then, 0.01 M Bi2O3 was added in both the anolyte and catholyte. The electrolyte flow rate for each half-cell was 30 mL min−1. The charge–discharge profiles of the Fe/Cu RFB were evaluated though a potential station (Solartron 1280C) at a current density of 20 mA cm−2 within a fixed potential range of 0–1.2 V.

3. Results and discussion

Fig. 2 depicts the CV curves of the Fe2+/Fe3+ redox couple using a GC electrode with various scan rates between −0.5 and 1.2 V (vs. Ag/AgCl) at room temperature. The current density was normalized to the geometrical area of the working electrode. As shown in the figure, increasing the scan rate from 10 to 70 mV s−1 results in an increase in the anodic and cathodic peak current densities. Moreover, the anodic peak potential that appears at about 0.68–0.78 V corresponds to the oxidation of Fe2+ to Fe3+. The corresponding cathodic peak potential occurs at about 0.23–0.33 V during the reverse scan. The redox peak potential separation related to the redox couple Fe2+/Fe3+ is around 0.4 V, indicating that the Fe2+/Fe3+ redox couple has sufficient reversibility to be used as the positive electrolyte for the proposed redox flow battery system.
image file: c7ra12926b-f2.tif
Fig. 2 CV curves of 1.5 M FeCl2 in a 3 M HCl using GC electrode at various scan rates.

To determine the potential region of the redox reactions, the CV curves of 1.8 M CuCl in 2.4 M HCl/2.4 M CaCl2 electrolyte solution were performed using a GC working electrode at different scan rates, as shown in Fig. 3, in which the potential window for Cu+/Cu0 and Cu2+/Cu+ was over 1.6 V. As observed, peak (a) displays the oxidation of Cu+ to Cu2+ and peak (b) shows the reduction of Cu2+ to Cu+. Peak (c) suggests the solid Cu formation on the GC electrode surface on the negative side. The sharp decrease in current indicates the typical nucleation loop related to the Cu metal electrodeposition onto the GC electrode. Once nucleation occurs, no difference is apparent between the various scan rates used. The final peak (d), suggests the dissolution of Cu0 that is electrodeposited onto the GC electrode, which oxidizes back to Cu+.


image file: c7ra12926b-f3.tif
Fig. 3 CV curves of 1.8 M CuCl in a mixed supporting electrolyte (2.4 M CaCl2 + 2.4 M HCl) solution using GC electrode at various scan rates.

To compare the electrochemical activities, a CV test was performed with and without the addition of Bi2O3. Fig. 4 presents the CV curves of the Fe2+/Fe3+ redox couple on a GC working electrode with and without the addition of Bi3+ at a scan rate of 50 mV s−1. The matching reactions of oxidation–reduction couples are marked in the figure. The standard potential of Bi3+/Bi0 (46 mV vs. Ag/AgCl) is detected in the CV curve along with that of the Fe2+/Fe3+ redox couple owing to the addition of Bi3+. The addition of Bi3+ ions has no influence on the oxidation–reduction reaction of Fe2+/Fe3+. This is because the Bi metal will be oxidized to Bi3+ ions prior to the oxidation of Fe2+ to Fe3+, indicating that Bi in the form of ions has no catalytic effect toward Fe2+/Fe3+ redox couple.25,26


image file: c7ra12926b-f4.tif
Fig. 4 CV curves of 1.5 M FeCl2 in a 3 M HCl using GC electrode with and without 0.01 M Bi3+ at a scan rate of 50 mV s−1.

Fig. 5 depicts the CV curves of 1.8 M CuCl in 2.4 M HCl/2.4 M CaCl2 electrolyte on a GC working electrode with and without adding Bi2O3 at a scan rate of 50 mV s−1. The corresponding redox pair reactions are marked in the figure. For the electrolyte without Bi3+, the peak potential separation corresponding to the Cu+/Cu2+ redox couple is 0.66 V. However, after the addition of 0.01 M Bi3+ to the electrolyte, the redox peak potential separation declines to 0.57 V. Moreover, in the case of Cu0/Cu+ redox couple, both oxidation and reduction peaks are clearly observed after adding Bi3+ as compared to the pristine electrolyte. This result indicates that after adding Bi3+, the copper redox couples have better electrochemical activity and reversibility. The reason is that the bismuth metal will be electrodeposited onto the negative GC electrode prior to the reduction of Cu2+ to Cu+, suggesting that the Bi metal in place of Bi3+ ions has a catalytic effect towards copper redox reactions.27,28 To investigate the catalytic effect of the Bi ions towards copper redox reactions, we measured the diffusion coefficients and rate constants for Cu0/Cu+ couple with and without adding Bi2O3. The results are listed in Table 1. The standard rate constant of Cu0/Cu+ with addition of Bi2O3 (7.33 × 10−4 cm s−1) is greater than that without adding Bi2O3 (4.87 × 10−4 cm s−1), indicating that Cu0/Cu+ with Bi2O3 has smaller overpotentials under the same conditions.19


image file: c7ra12926b-f5.tif
Fig. 5 CV curves of 1.8 M CuCl in a mixed supporting electrolyte (2.4 M CaCl2 + 2.4 M HCl) solution using GC electrode with and without 0.01 M Bi3+ at a scan rate of 50 mV s−1.
Table 1 Comparison of the diffusion coefficients and rate constants for Cu0/Cu+ couple with and without adding Bi2O3
Parameters Without Bi3+ With 0.01 M Bi3+
Diffusion coefficient (DO) 7.40 × 10−8 cm2 s−1 1.74 × 10−7 cm2 s−1
Rate constant (k0) 4.87 × 10−4 cm s−1 7.33 × 10−4 cm s−1


A charge–discharge cycling performance test was conducted using a Fe/Cu RFB single cell with Nafion 117 as a membrane to demonstrate the effect of the carbon electrode on the electrochemical performance of the Fe/Cu RFB cell. Fig. 6 presents the charge–discharge profiles for the cells with microwave heat treated GF (HT-GF) and microwave heat treated GF + microwave heat treated one layer CP (HT-GF + HT-CP) electrodes at a constant current density of 20 mA cm−2. The VRFB cell with the HT-GF + HT-CP electrode exhibits a longer charge–discharge time, lower charge voltage plateau, and higher discharge voltage plateau than the HT-GF, which results in higher energy and voltage efficiency. This is because more oxygen-containing functional groups are introduced onto the carbon fiber surface during the microwave pretreatment process,29,30 which can facilitate the Fe2+/Fe3+and Cu+/Cu0 redox reactions. Moreover, in the case of the HT-GF + HT-CP electrode, the subsequent electrodeposition of Cu metal onto the GF surface is lower, as shown in the ESI (Fig. S1b), leading to higher discharge and lower charge voltage.6,31 The CE, EE, and VE data obtained from Fig. 6 are listed in Table 2.


image file: c7ra12926b-f6.tif
Fig. 6 Charge–discharge curves of Fe/Cu RFB cells with HT-GF and HT-GF + HT-CP at a current density of 20 mA cm−2.
Table 2 Summary of the efficiencies of two cells obtained at 20 mA cm−2
Cells with CE (%) EE (%) VE (%)
HT-GF 88.77 21.05 23.71
HT-GF + HT-CP 84.10 34.43 40.94


To further investigate the effect of adding Bi3+ in the electrolytes on the performance of the Fe/Cu RFB single cell, charge/discharge cycling curves were recorded with and without 0.01 M Bi3+. Fig. 7 shows the charge–discharge curves of a Fe/Cu RFB in the absence and presence of Bi3+ in the electrolytes at a current density of 20 mA cm−2. The CE, EE, and VE data obtained from the curves shown in Fig. 7 are listed in Table 3. It is found that the cell containing Bi3+ in electrolytes reveals higher CE and EE than the cell without Bi3+. This is because after adding Bi3+, no Cu metal precipitation was observed on the electrode surface (see Fig. S1c), which indicated that the electrodeposition process was potentially reversible on the electrode material.


image file: c7ra12926b-f7.tif
Fig. 7 Charge–discharge curves of a Fe/Cu RFB with and without 0.01 M Bi3+ in the electrolytes at a current density of 20 mA cm−2.
Table 3 Summary of the efficiencies of two cells obtained at 20 mA cm−2
Cells with CE (%) EE (%) VE (%)
HT-GF + HT-CP 84.10 34.43 40.94
HT-GF + HT-CP + 0.01 M Bi3+ 89.18 35.24 39.52


Fig. 8a presents charge–discharge cycling curves of a Fe/Cu RFB with 0.01 M Bi3+ in the electrolytes at 20 mA cm−2. The resultant efficiencies obtained from Fig. 8a as a function of cycle number are plotted in Fig. 8b. As can be observed in Fig. 8b, the efficiencies of the battery are stable over 10 cycles, which demonstrates that Fe/Cu RFB has good stability on the HT-GF + HT-CP electrode after adding Bi3+ in the electrolytes.


image file: c7ra12926b-f8.tif
Fig. 8 (a) Charge–discharge cycling curves and (b) stability test of the Fe/Cu RFB with 0.01 M Bi3+ at a current density of 20 mA cm−2.

In brief, we propose a novel, abundant, low-cost, and environmentally benign Fe/Cu RFB, which employs Fe2+/Fe3+ and Cu+/Cu0 as the positive and negative electrolytes, respectively. We investigated the effect of GF electrode modification and the addition of Bi3+ in the electrolytes on the charge–discharge performance of the Fe/Cu RFB. The results confirmed that the cell containing Bi3+ in electrolytes revealed higher CE (89.18%) and EE (35.24%) than the cell without Bi3+ (CE = 84.10% and EE = 34.43%) at a current density of 20 mA cm−2. This is because the presence of Bi3+ avoids precipitation of Cu metal on the electrode surface, which indicates that the electrodeposition process is potentially reversible on the electrode material, thus leading to enhanced performance of the battery.

Cost is probably the most important and fundamental issue of energy storage systems for a broad market penetration. The key costs of RFBs are the active material stored in the electrolyte and the electrochemical cell.32 Therefore, we considered only the electrolyte and stack material costs, while the cost of the remaining balance-of-plant was not considered. In the case of Fe/Cu RFB, we estimate that the cost of the electrolyte is around $33 (kW h)–1 of energy storage, which is much lower than that in the VRFB system. Considering the price of the materials used in the stack, we estimate that the stack has a price of around $100–150 m−2, which corresponds to a system cost of $170–230 (kW h)−1. The VRFB, which is the most developed aqueous RFB, is estimated to have a vanadium material cost of $189 (kW h)−1 and a system cost of $325 (kW h)−1.6 By considering these values, in combination with the lower electrolyte cost we place the Fe/Cu RFB system well ahead of the VRFB in terms of attractiveness for practical applications.

As we already estimated, the system cost of Fe/Cu RFB is about $170–230 (kW h)−1, while Li-ion batteries, for example, have a system cost about $400–600 (kW h)−1,1 which is clearly still too high for broad market penetration. The high cost is primarily attributed to the high cost of materials (lithium). Hence, Li-ion batteries are more expensive than Fe/Cu RFB. In general, for stationary applications, the Li-ion batteries of current interest for vehicle applications may face a few challenges. First and foremost, the cost of the Li-ion batteries that are targeted for vehicle applications is 2–5 times higher on a kW h basis than that for the stationary applications.33 In addition, the targeted performance parameters of the Li-ion batteries may not be good enough for stationary applications. For example, stationary applications generally require a longer cycle and calendar life than that for vehicle applications. A further challenge of Li-ion batteries for stationary applications is in safety and reliability. As for transportation applications, the Li-ion batteries must be safe and reliable. This becomes particularly important for grid applications for scale-up to MW levels.

4. Conclusions

In summary, a novel, abundant, low-cost, and environmentally benign Fe/Cu RFB on the basis of Fe2+/Fe3+ redox couple as the positive electrolyte and Cu+/Cu0 redox couple as the negative electrolyte in a flow cell was successfully developed for large-scale energy storage applications. The effect of GF electrode modification and addition of Bi3+ in the electrolytes on the charge–discharge performance of the Fe/Cu RFB were investigated. The results confirm the following. (1) The VRFB cell with the HT-GF + HT-CP electrode exhibited longer charge–discharge time, lower charge voltage plateau, and higher discharge voltage plateau than the HT-GF, which results in higher energy and voltage efficiency. This is because more oxygen-containing functional groups were introduced on the carbon fibers surface during the microwave pretreatment process, which facilitated the Fe2+/Fe3+ and Cu+/Cu0 redox reactions. (2) The cell containing Bi3+ in electrolytes reveals higher CE (89.18%) and EE (35.24%) than the cell without Bi3+ (CE = 84.10% and EE = 34.43%) at a current density of 20 mA cm−2. This is because the presence of Bi3+ avoids precipitation of Cu metal on the electrode surface, which indicates that the electrodeposition process is potentially reversible on the electrode material, thus leading to enhanced performance of the battery. Furthermore, the efficiencies of the battery are stable over 10 cycles, which demonstrates that Fe/Cu RFB has good stability on the HT-GF + HT-CP electrode after adding Bi3+ in the electrolytes. However, the energy efficiency of our proposed battery is still low. Further investigation is still needed to improve the energy efficiency by optimizing parameters such as the electrolytes' composition, cell component materials, and operating temperatures.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This research is supported by the Institute of Nuclear Energy Research, Atomic Energy Council. We would like to acknowledge Prof. Kuei-Hsien Chen at Academia Sinica and Prof. Li-Chyong Chen at National Taiwan University (NTU) for their helpful assistance.

References

  1. G. L. Soloveichik, Chem. Rev., 2015, 115, 11533–11558 CrossRef CAS PubMed.
  2. L. Li, S. Kim, W. Wang, M. Vijayakumar, Z. Nie, B. Chen, J. Zhang, G. Xia, J. Hu, G. Graff, J. Liu and Z. Yang, Adv. Energy Mater., 2011, 1, 394–400 CrossRef CAS.
  3. W. Wang, Z. Nie, B. Chen, F. Chen, Q. Luo, X. Wei, G.-G. Xia, M. Skyllas-Kazacos, L. Li and Z. Yang, Adv. Energy Mater., 2012, 2, 487–493 CrossRef CAS.
  4. D. M. Kabtamu, J.-Y. Chen, Y.-C. Chang and C.-H. Wang, J. Mater. Chem. A, 2016, 4, 11472–11480 CAS.
  5. D. M. Kabtamu, J.-Y. Chen, Y.-C. Chang and C.-H. Wang, J. Power Sources, 2017, 341, 270–279 CrossRef CAS.
  6. Y. K. Zeng, X. L. Zhou, L. An, L. Wei and T. S. Zhao, J. Power Sources, 2016, 324, 738–744 CrossRef CAS.
  7. K. Lin, Q. Chen, M. R. Gerhardt, L. Tong, S. B. Kim, L. Eisenach, A. W. Valle, D. Hardee, R. G. Gordon, M. J. Aziz and M. P. Marshak, Science, 2015, 349, 1529–1532 CrossRef CAS PubMed.
  8. B. Huskinson, M. P. Marshak, C. Suh, S. Er, M. R. Gerhardt, C. J. Galvin, X. Chen, A. Aspuru-Guzik, R. G. Gordon and M. J. Aziz, Nature, 2014, 505, 195–198 CrossRef CAS PubMed.
  9. B. Li, Z. Nie, M. Vijayakumar, G. Li, J. Liu, V. Sprenkle and W. Wang, Nat. Commun., 2015, 6, 6303 CrossRef CAS PubMed.
  10. K. Lin, R. Gómez-Bombarelli, E. S. Beh, L. Tong, Q. Chen, A. Valle, A. Aspuru-Guzik, M. J. Aziz and R. G. Gordon, Nat. Energy, 2016, 1, 16102 CrossRef CAS.
  11. J. Noack, N. Roznyatovskaya, T. Herr and P. Fischer, Angew. Chem., Int. Ed. Engl., 2015, 54, 9776–9809 CrossRef CAS PubMed.
  12. H. Haller and S. Riedel, Z. Anorg. Allg. Chem., 2014, 640, 1281–1291 CrossRef CAS.
  13. G. C. M. Lopez-Atalaya, J. R. Perez, J. L. Vazquez and A. Aldaz, J. Power Sources, 1992, 39, 147–154 CrossRef.
  14. E. Sum, M. Rychcik and M. Skyllas-kazacos, J. Power Sources, 1985, 16, 85–95 CrossRef CAS.
  15. A. Parasuraman, T. M. Lim, C. Menictas and M. Skyllas-Kazacos, Electrochim. Acta, 2013, 101, 27–40 CrossRef CAS.
  16. M. Park, Y.-J. Jung, J. Kim, H. I. Lee and J. Cho, Nano Lett., 2013, 13, 4833–4839 CrossRef CAS PubMed.
  17. R. F. Savinell and L. W. Hruska, J. Electrochem. Soc., 1981, 128, 18–25 CrossRef.
  18. T. J. Petek, N. C. Hoyt, R. F. Savinell and J. S. Wainright, J. Power Sources, 2015, 294, 620–626 CrossRef CAS.
  19. K. Gong, F. Xu, J. B. Grunewald, X. Ma, Y. Zhao, S. Gu and Y. Yan, ACS Energy Lett., 2016, 1, 89–93 CrossRef CAS.
  20. T. S. Zhao, Y. K. Zeng, L. An, X. L. Zhou and L. Wei, J. Power Sources, 2015, 300, 438–443 CrossRef.
  21. L. Sanz, D. Lloyd, E. Magdalena, J. Palma, M. Anderson and K. Kontturi, J. Power Sources, 2015, 278, 175–182 CrossRef CAS.
  22. L. Sanz, J. Palma, E. García-Quismondo and M. Anderson, J. Power Sources, 2013, 224, 278–284 CrossRef CAS.
  23. P. Leung, J. Palma, E. Garcia-Quismondo, L. Sanz, M. R. Mohamed and M. Anderson, J. Power Sources, 2016, 310, 1–11 CrossRef CAS.
  24. D. Lloyd, E. Magdalena, L. Sanz, L. Murtomäki and K. Kontturi, J. Power Sources, 2015, 292, 87–94 CrossRef CAS.
  25. B. Li, M. Gu, Z. Nie, Y. Shao, Q. Luo, X. Wei, X. Li, J. Xiao, C. Wang, V. Sprenkle and W. Wang, Nano Lett., 2013, 13, 1330–1335 CrossRef CAS PubMed.
  26. L. Wei, T. S. Zhao, L. Zeng, X. L. Zhou and Y. K. Zeng, Applied Energy, 2016, 180, 386–391 CrossRef CAS.
  27. T. Liu, X. Li, H. Nie, C. Xu and H. Zhang, J. Power Sources, 2015, 286, 73–81 CrossRef CAS.
  28. D. J. Suarez, Z. Gonzalez, C. Blanco, M. Granda, R. Menendez and R. Santamaria, ChemSusChem, 2014, 7, 914–918 CrossRef CAS PubMed.
  29. X. Wu, H. Xu, P. Xu, Y. Shen, L. Lu, J. Shi, J. Fu and H. Zhao, J. Power Sources, 2014, 263, 104–109 CrossRef CAS.
  30. Y. K. Zeng, T. S. Zhao, X. L. Zhou, L. Zeng and L. Wei, Applied Energy, 2016, 182, 204–209 CrossRef CAS.
  31. L. Sanz, D. Lloyd, E. Magdalena, J. Palma and K. Kontturi, J. Power Sources, 2014, 268, 121–128 CrossRef CAS.
  32. M. M. M., A. Z. Weber, J. P. Meyers, P. N. Ross, J. T. Gostick and Q. Liu, J. Appl. Electrochem., 2011,(41), 1137 Search PubMed.
  33. Z. Yang, J. Zhang, M. C. Kintner-Meyer, X. Lu, D. Choi, J. P. Lemmon and J. Liu, Chem. Rev., 2011, 111, 3577–3613 CrossRef CAS PubMed.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra12926b

This journal is © The Royal Society of Chemistry 2018
Click here to see how this site uses Cookies. View our privacy policy here.