Self-assembled nanoribbons from small molecule amphiphiles with a structural domain to impart mechanical stability and chelating head groups are reported for the remediation of lead from contaminated water. The nanoribbons' remediation capacity is affected by pH and the presence of competing cations, and can be modulated by head group choice.
Environmental significanceLead poisoning causes over one million deaths annually, leading to the designation of lead as one of the World Health Organization's “ten chemicals of major public health concern”. To address this crisis, high surface area nanomaterials offer promise for producing miniaturized technologies capable of effective lead remediation. We present small molecules that spontaneously self-assemble in water to form nanoribbons with lead-chelating surface groups. While supramolecular nanostructures are typically fragile, we incorporate hydrogen bonding aramid domains to suppress exchange dynamics, ultimately leading to nanoribbons with structural integrity. We demonstrate that design of small molecules is a route to new ion-selective chelating nanomaterials with tunable surface chemistries, and thereby demonstrate the potential of small molecule self-assembly for heavy metal remediation. |
Molecular self-assembly could offer notable advantages to applications in non-biological contexts if their typical dynamic instabilities were overcome. In particular, self-assembled nanomaterials may provide a new strategy for point-of-use remediation of contaminants from drinking water. Surface areas on the order of hundreds of m2 g−1 – resulting from nanostructure length scales determined by the length of the constituent amphiphiles1,14 – may provide a platform for sequestering heavy metals. Namely, these nanostructure surfaces could be entirely coated with moieties capable of heavy metal remediation by presenting a hydrophilic chelator on every molecule. Realizing this design rationale requires the suppression of amphiphile exchange to minimize the rearrangement and release of amphiphile molecules from their assembled structures into the solvent space. Suppression of these exchange dynamics may also reduce the sensitivity of the assembly to variations in its environment such and temperature and pH.15
The removal of lead ions, Pb2+, from drinking water is a critical target. Inorganic lead is a potent toxin which can damage nearly all organs, with adverse health effects including neurotoxicity, cardiovascular complications, cancer, and death.16,17 Lead enters drinking water from a variety of sources, including the production and disposal of lead-acid batteries, alloy manufacturing, and, particularly, the erosion of plumbing.18–20 Lead contamination crises persist globally, and increasing research indicates these events disproportionately occur in the United States along racial and socioeconomic lines.21–24 Thus, there exists an urgent need to develop contemporary strategies for point-of-use remediation of lead from drinking water streams.
Here, we present the design of small molecule amphiphiles which exhibit three characteristics for the remediation of lead from contaminated water (Fig. 1): (1) amphiphilicity to induce spontaneous self-assembly in water into high surface area nanostructures; (2) a structural domain to provide intermolecular cohesion; and (3) a chelating head group capable of strongly binding to heavy metal cations in solution. To accomplish these goals, we use the aramid amphiphile (AA) motif as the platform for molecular self-assembly.25,43 AAs take advantage of a dense hydrogen bonding network to impart structural stability on assembled nanoribbons with surface areas on the order of 200 m2 g−1. Of particular note for this application, the amphiphiles exhibit suppressed exchange dynamics upon assembly, hindering the release of amphiphiles from their nanostructure. The supressed exchange dynamics differentiate this self-assembly approach from those that have been previously explored for water treatment.26,27 In previous reports, heavy metal cations initiate physical crosslinking that induces hydrogelation – a process that may impede surface chelation events by limiting diffusion to the inside of the gel.28 This design presents advantages over other soft materials systems, including polymers and polymer networks, because: (1) all chemical groups responsible for heavy metal remediation are expressed on the nanostructure surfaces, and are thermodynamically prohibited from being buried within a material; (2) surface chemistries and functionalities can be readily tuned through careful selection of the hydrophilic head group, enabling tuning of heavy metal remediation effectiveness and selectivity; and (3) the chemical character of the chelating compounds is minimally impacted by requiring only one covalent tether to the nanostructure surface, maximizing ionic interactions with dissolved lead species.
We designed and synthesized two AAs for the remediation of heavy metals from drinking water: compound 1, an AA with a DOTA (dodecane tetraacetic acid; also known as tetraxetan) head group, and compound 2, an AA with a DTPA (diethylenetriaminepentaacetic acid; also known as pentetic acid) head group (Fig. 1a). These groups were selected for their high binding affinity to lead ions in solution and their capability of inducing amphiphilic self-assembly by providing sufficient head group hydrophilicity (Fig. 1b). Both AAs with DOTA and DTPA head groups harness ionic interactions from charged carboxylic acid moieties and dipole interactions from tertiary amines to sequester lead ions from water.29,30 Compounds 1 and 2 were obtained by alternating carbodiimide-mediated amidation reactions and standard deprotection reactions. Synthesis details and characterization of the final compounds and their intermediates are provided in ESI† section 1.
We observe the spontaneous assembly of both compounds 1 and 2 in water into nanoribbons with lengths extending at least several microns (Fig. 2a and c) by transmission electron microscopy (TEM). To ascertain cross-sectional dimensions, we use cryogenic TEM (Cryo-TEM) to obtain high-resolution images of the nanoribbons in a solvated state and synchrotron small angle X-ray scattering (SAXS) for nanostructure characterization. From these techniques, we find a 3.9 nm thickness and 8.8 nm width for compound 1, and a 3.9 nm thickness by 5.1 nm width for compound 2 (Fig. 2b and d and ESI† Fig. S1). These dimensions give rise to surfaces areas on the order of 200 m2 g−1.25
Having identified the geometries of the self-assembled nanostructures, we use a variety of techniques to characterize the chelation performance of compound 1 nanoribbons. Ultraviolet-visible (UV-vis) absorption spectroscopy allows us to observe the formation of the DOTA-lead complex.31 An absorption peak at λ = 262 nm, characteristic of this complex, emerges as lead ions are titrated into a solution of compound 1 nanoribbons (Fig. 3a). The rise of this peak plateaus at 50 mol% Pb2+, most likely signifying a 2:1 complexation of DOTA to the lead ions. This sandwich-type complex has been previously observed in similar systems where cyclic chelating moieties are maintained in close proximity.32
We employ isothermal titration calorimetry (ITC) to quantify thermodynamic parameters of the lead-binding surface reaction (Fig. 3b). This experiment captures the heat released from the injection of a concentrated lead solution into a dilute nanoribbon suspension. Injection of the concentrated lead solution into nanoribbon-free water is background-subtracted from this data to remove the heat of dilution. Negligible signal is detected by the injection of water into the nanoribbon suspension. From fitting sigmoidal curves to n = 3 runs, we calculate an equilibrium binding constant Kb = 2.2 ± 0.5 × 105 M−1. This value indicates an equilibrium which strongly prefers the binding of lead ions to the nanoribbon surfaces, rather than the presence of lead ions free in solution, and implies that the nanoribbons are successful in remediating the heavy metal from contaminated water. This equilibrium constant further suggests that compound 1 nanoribbons should be used in significant excess to the lead present in contaminated water to thermodynamically drive remediation below the 15 ppb regulatory level for toxicity.16 We further observe the plateau of chelation signal at n = 0.5, corroborating the saturation of the nanoribbons at 50 mol% Pb, and that the nanoribbons maintain their morphology after lead chelation (ESI† Fig. S2).
We hypothesize that the remediation capacity of lead ions by AA nanoribbons should be affected by pH, as protonation of the nanoribbon head groups would hinder ionic interactions between the chelating moieties and lead ions.33 Because lead species become insoluble in basic environments,34 we selected pH values of 7, 5, and 3 to test remediation capacity. We observe no change in assembly morphology of compound 1 nanoribbons when the pH is adjusted to 3 post-assembly (ESI† Fig. S3), likely because of the stability imparted to the structure by the aramid domain.
Adsorption isotherm curves are constructed for the uptake of lead by compound 1 nanoribbons to test pH sensitivity (Fig. 3c). Nanoribbons are mixed with Pb2+ 24 h before testing to ensure equilibrium is reached. Equilibrium data are fit to a Langmuir model, with R2 values exceeding 0.97 in all cases (ESI† Fig. S4). Compound 1 nanoribbons demonstrate adsorption capacities (Qo) of 72, 61, and 45 mg g−1 at pH values of 7, 5, and 3, respectively. As predicted, the lead chelation capacity drops slightly when changing from pH 7 to 5, and drops significantly at pH 3.
We further expect that the nanoribbons' lead adsorption capacities is sensitive to the presence of other multivalent cations which could compete with lead to occupy the chelation complex. To test this hypothesis, we constructed adsorption isotherms with equimolar amounts of lead and either calcium, copper, magnesium, or nickel ions (Fig. 3d). Fits of the equilibrium data to a Langmuir model (ESI† Fig. S5) are used to extract lead adsorption capacities in the equimolar presence of each ion: for Ca2+, Qo,Pb2+ = 61 mg g−1; for Mg2+, Qo,Pb2+ = 52 mg g−1; for Cu2+, Qo,Pb2+ = 32 mg g−1; and for Ni2+, Qo,Pb2+ = 27 mg g−1. Thus, from least to most interference with Pb2+ binding to compound 1 nanoribbons, we observe the following trend: Ca2+ < Mg2+ ≪ Cu2+, Ni2+. This trend largely follows the equilibrium binding constants of the ions to the free DOTA molecule in solution.35 To put this data in perspective, remediating 1 L of water with 50 ppb Pb to below 15 ppb Pb at pH 7 requires approximately 690 μg of compound 1 nanoribbons in the absence of competing counterions, and 820, 960, 1560, and 1850 μg compound 1 nanoribbons in the presence of equimolar amounts of Pb2+ and Ca2+, Mg2+, Cu2+, and Ni2+, respectively. These results confirm that the lead-binding capacity of compound 1 nanoribbons is reduced by the presence of competing multivalent cations and suggests that this system may be used to simultaneously remove several contaminants from polluted water.
The capacity of amphiphilic nanoribbons to remediate heavy metal ions from water should be sensitive to the geometry and chemical structure of the head group.33 Lead ions likely percolate into the head group domain of compound 1 to sandwich between neighbouring DOTA head groups. Conversely, the DTPA head group of compound 2 is prone to facing outwards from the nanoribbon core due to steric hinderance and has four carboxylic acids per molecule available for complexation. Therefore, we expect compound 2 nanoribbons to exhibit more effectively sequester Pb2+ from water than those of compound 1.
The formation of a lead:amphiphile chelation complex on compound 2 nanoribbons is monitored by UV-vis absorption spectroscopy with the emergence of a peak at λ = 255 nm (Fig. 4a). We observe that compound 2 nanoribbons maintain their morphology with chelation (Fig. S2†) and, interestingly, find compound 2 nanoribbon chelators saturate near 50 mol% Pb. This effect may result from hydrogen bonding between head groups, which leads to the bundling of nanoribbons (Fig. 2c and d), reducing the effective accessible surface area. Compound 2 nanoribbons exhibit an equilibrium binding constant of Kb = 7.1 ± 1.6 × 105 M−1 in n = 3 background-subtracted ITC experiments (Fig. 4b). This binding constant is statistically significantly higher than that of compound 1, and predicts that compound 2 nanoribbons should thus exhibit enhanced lead binding in adsorption isotherm experiments. As with compound 1 nanoribbons, this equilibrium constant also implies that achieving lead remediation below 15 ppb requires using a significant excess of compound 2 nanoribbons relative to the lead present in the water.16
As with compound 1, the remediation capacity of compound 2 nanoribbons is expected to be sensitive to pH as head group protonation inhibits ionic interactions with lead ions (Fig. 4c and ESI† Fig. S6). Compound 2 nanoribbons are also demonstrated to maintain their nanostructure upon environmental adjustment to pH 3 (ESI† Fig. S3). At pH 7, compound 2 nanoribbons have an equilibrium saturation capacity of Qo = 96 mg g−1. This saturation capacity drops slightly to Qo = 93 mg g−1 at pH 5, and further declines to Qo = 81 mg g−1 at pH 3, following the expected trend and matching the pattern of compound 1. Notably, the saturation capacity of compound 2 nanoribbons is higher than those of 1 across all pH values. This result, in conjunction with the elevated thermodynamic equilibrium binding constant of 2 nanoribbons, confirms that head group choice is a viable parameter for tuning chelation capacity of small molecule amphiphilic nanoribbons.
The saturation capacities of the nanoribbon materials presented here match or exceed those of functional materials investigated or in use today for lead remediation. For example, the equilibrium saturation capacities of compound 1 and 2 nanoribbons exceed that of activated carbon (50 mg g−1),36 sulfur-functionalized silica (46 mg g−1),37 acidified carbon nanotubes (17 mg g−1),38 and apricot stone (21 mg g−1).39 In contrast, compound 1 and 2 nanoribbons offer comparable performance to Fe(III)-modified zeolite (99 mg g−1)40 and iron oxide nanomaterials (98 mg g−1).41
Finally, we sought to identify the effect of competitive binding for chelation sites by divalent cations on compound 2 nanoribbons. We again performed adsorption isotherm experiments with equimolar amounts of lead and either calcium, copper, magnesium, or nickel ions (Fig. 4d and ESI† Fig. S7). For compound 2 nanoribbons, we find for Ca2+, Qo,Pb2+ = 96 mg g−1; for Mg2+, Qo,Pb2+ = 90 mg g−1; for Ni2+, Qo,Pb2+ = 42 mg g−1; and for Cu2+, Qo,Pb2+ = 34 mg g−1. From least to most interference with Pb2+ binding to 2 nanoribbons, we observe: Ca2+ < Mg2+ ≪ Ni2+ < Cu2+. These results indicate that remediating 1 L of water with 50 ppb Pb to below 15 ppb Pb at pH 7 requires approximately 520 μg of compound 2 nanoribbons in the absence of competing counterions, and 520, 560, 1190, and 1470 μg compound 2 nanoribbons in the presence of equimolar amounts of Pb2+ and Ca2+, Mg2+, Ni2+, and Cu2+, respectively. This trend generally follows that of equilibrium binding constants for these ions to free DTPA in solution.35 Fractionally and in total saturation magnitude, compound 2 is affected less by competitive binding with these cations than compound 1, with the exception of copper(II). This result suggests that head group choice can be used not only to improve adsorption capacity, but also to tune ion selectivity.
Footnote |
† Electronic supplementary information (ESI) available: Synthesis and experimental details, Fig. S1–S7. See DOI: 10.1039/d1en00002k |
This journal is © The Royal Society of Chemistry 2021 |