Zinc-diffused silver indium selenide quantum dot sensitized solar cells with enhanced photoconversion efficiency

Ganga Halder and Sayan Bhattacharyya *
Department of Chemical Sciences and Centre for Advanced Functional Materials, Indian Institute of Science Education and Research (IISER) Kolkata, Mohanpur-741246, India. E-mail: sayanb@iiserkol.ac.in

Received 9th January 2017 , Accepted 17th February 2017

First published on 20th February 2017


Abstract

Alloying of quantum dots (QDs) with suitable metal ions is one of the efficient tools to enhance the power conversion efficiency (PCE) of QD sensitized solar cells (QDSSCs). Ternary AgInX2 (X = S, Se) based liquid-junction QDSSCs have low PCEs due to the presence of defect states at internal atom vacancies. However, Zn2+ diffusion at these vacant sites can improve the carrier mobility of the QDs. The QDSSCs with Zn2+-diffused AgInSe2 (ZAISE) QDs have a broad light harvesting range up to the near-infrared (NIR) range. PCE was enhanced from a merely 1.67% for pristine AgInSe2 QDs (AISE) to 3.07% for ZAISE with a Zn/(Ag + In) ratio of 48.2%, aided by an optimized ZnS passivation layer on the photoanode. The device efficiency was further improved to 3.57% by applying dual passivation of amorphous TiO2 and SiO2 layers. This approach could effectively suppress the recombination pathways at the QD surface and thereby minimize back electron transfer from photoexcited electrons of QDs and from the conduction band of TiO2 to the polysulfide electrolyte. The combined strategy of alloying with Zn2+ and inorganic passivation could achieve the highest ever PCE of environmentally friendly AgInX2 based QDSSCs.


1. Introduction

Semiconductor QDs have size-controllable photophysical properties such as the tunability of their band gap, a high absorption coefficient, an ability to generate multiple excitons by a single photon and a large carrier lifetime which offers the possibility of boosting the PCE of photovoltaic devices beyond the Shockley–Queisser limit.1–5 In QDSSCs, narrow band gap cadmium and lead based chalcogenide semiconductors like CdS, CdSe, PbS, and PbSe are popularly employed as sensitizers and wider band gap metal oxide semiconductors like TiO2, ZnO and SnO2 are used as electron acceptors.6 However, the low to moderate PCE of these binary QDs lingers due to their limited light harvesting range and/or poor charge injection efficiency. In comparison, alloyed QDs are superior substitutes since their band gap can be tuned by changing their composition to obtain a broad light harvesting range and suitable band gap alignment for effective charge injection.7 Recently, copper and silver based ternary QDs have received attention for the fabrication of third generation photovoltaic devices due to their broad light harvesting range from the UV-visible to the NIR region. This broad range is very crucial for capturing a large number of solar photons. More importantly, these ternary alloyed QDs are free from toxic elements such as cadmium and lead which will open a new window for the commercial application of “non-toxic” QDs in QDSSCs for future environmental prospects.8–10

Although ternary alloyed QDs are good light harvesters, the efficiency of the photovoltaic devices is limited due to their high density of trap states which act as recombination centers in QDSSCs.10–12 AgInSe2 (AISE) is a I-III-VI2 semiconductor having a direct bulk band gap of 1.19 eV, which is ideal for solar cell applications attributed to its high absorption coefficient. Although it has a broad light harvesting range, several vacancies at Ag and Se lattice sites along with internal atom vacancies lead to defect states.13,14 In order to improve the PCE, silver chalcogenides were manipulated through creation of Ag2S–AgInS2 based p–n junction heterostructures15,16 and AgInS2 QDs/In2S3 based photoelectrodes,17 or introducing a buffer layer between AgInS2 QD sensitizers and ZnO nanorod arrays.18 In spite of several efforts, the device efficiency is still low. The presence of defect states reduces the crystallinity, electrical conductivity and carrier mobility in ternary QDs. These trap states with a high density also act as recombination centers, thereby decreasing the photovoltage and photovoltaic performance.19,20 One of the ways to reduce the density of surface trap states is surface modification of ternary QDs where the passivation layers act as a barrier to minimize the electron and hole transfer rates.8,9,21

The diffusion of foreign metal ions into the vacant sites of ternary QD lattices is another suitable approach to improve the conductivity as well as PCE by minimizing the prevalent defect states. For example, Cu-diffused AISE QDs in organic/inorganic bulk-heterojunction devices decrease the internal resistance and increase the short-circuit current density (JSC) under white light illumination.22 These alloying strategies alter the energy difference (ΔECB) between the conduction energy levels of the QDs and metal oxide, henceforth increasing the injection efficiency of the photogenerated electrons. If ΔECB is large enough, then photogenerated electrons can be rapidly injected into the metal oxide to enhance the charge collection efficiency and PCE.23 Although QDSSCs with ternary alloyed Zn–CuInSe2 QD sensitizers have already achieved 11.6% PCE through manipulation of the conduction band energy level,24 the breakthrough in AISE QD sensitized QDSSCs is much in demand to achieve improved PCE by increasing the crystallinity and carrier mobility of the QDs as well as by applying appropriate surface passivation.

In this work, Zn2+-diffused AgInSe2 (ZAISE) QDs with a broad light harvesting range from visible to NIR were synthesized by a hot injection method. The chemical composition of the QDs was varied by altering the ratio of Zn/(Ag + In). Higher Zn diffusion increases the ZAISE band gap. Through different optimization steps, the best PCE obtained is 3.57% when the Zn/(Ag + In) at% is 48.2. Our strategy could enhance the PCE of these “non-toxic” QDSSCs by ∼23% as compared to previous attempts.

2. Results and discussion

2.1 Characterization of the QDs

2.1.1 Structural characterization. A two-step in one pot synthetic procedure was employed for the preparation of ZAISE QDs. In the first step, the Ag2Se QDs were synthesized within 3 min at 88 °C from the reaction between Ag-oleylamine complex solution with very reactive phosphine-free Se-precursor. The Se-precursor was obtained from the reduction of Se powder by a 1[thin space (1/6-em)]:[thin space (1/6-em)]1 mixture of oleylamine and dodecanethiol. The Ag2Se QDs crystallize in the orthorhombic crystal structure according to JCPDS pattern 24-1041 (Fig. S1). Thereafter the reaction mixture was further heated to 180 °C for the diffusion of In3+ and Zn2+ into the Ag2Se crystal lattice to form ZAISE QDs. Since the ionic radii of In3+ and Zn2+ are 1.44 and 0.68 Å, respectively, these ions can easily diffuse into the vacant sites of Ag2Se where the ionic radius of Ag+ is 1.54 Å.25,26 The QD samples denoted as AZ0, AZ4, AZ5 and AZ6 have a Zn:(Ag + In) at% of 0, 36, 48 and 58, respectively, as obtained by inductively coupled plasma mass spectrometry (ICP-MS) analyses. The powder X-ray diffraction (XRD) patterns in Fig. 1a show that all the QDs crystallize in the tetragonal crystal structure (Fig. 1b) with space group I[4 with combining macron]2d according to the JCPDS pattern 75-0118. ICP-MS data show that on moving from AZ0 to AZ5, the drop in Ag:(Ag + In + Zn) is 30% whereas that of In:(Ag + In + Zn) is 70%. Therefore it is evident that a majority of Zn2+ sits in the In3+ sites than at Ag+ sites, and the relatively closer ionic radii of In3+ and Zn2+ are another validation to this argument. Also, the simultaneous diffusion of In3+ and Zn2+ in the Ag2Se lattice provides a competition between them to occupy the lattice vacancies. The crystallite size of the QDs is 3.2–3.5 nm which is calculated from the powder XRD pattern of the QDs using the Debye–Scherrer equation after subtracting the instrumental broadening. The representative transmission electron micrographs (TEMs) show that the particle size of the monodisperse QDs is around 4–6 nm with a moderately narrow size distribution (Fig. 1c and e). The AISE and ZAISE QDs were ligand-exchanged by replacing the initial hydrophobic oleylamine surfactant with mercaptopropionic acid (MPA) in order to obtain a maximum loading of the QDs on the TiO2 substrate and improve the film conductivity of QDSSCs.27 The interplanar spacing shows the high crystallinity and the indexed fast Fourier transform (FFT) patterns (Fig. 1d and f) confirm the purity of the as-synthesized QDs.
image file: c7ta00268h-f1.tif
Fig. 1 (a) Powder XRD patterns of the QDs. (b) Representative unit cell of AZ5. (c) Low resolution TEM image of AZ0 with the diameter histogram as the inset. (d) High resolution TEM image of AZ0 with the FFT pattern as the inset. (e) Low resolution TEM image of AZ5 with the diameter histogram as the inset. (f) High resolution TEM image of AZ5 with the FFT pattern as the inset.
2.1.2 Optical characterization. The absorption spectra of all the QDs synthesized at 180 °C (Fig. 2a and S2) show a broad light harvesting range from visible to NIR, an essential requirement to achieve high efficiency QDSSCs. The band gap of AZ0, AZ4, AZ5 and AZ6 is 1.50, 1.50, 1.53, and 1.56 eV as measured from the Tauc plots (Fig. S3a). To evaluate the impact of synthesis temperature and resultant particle size on the band gap, the absorption spectra of AZ5 QDs were recorded with the aliquots at different reaction temperatures. Fig. 2b shows the reaction temperature dependent UV-Vis-NIR spectra of AZ5 QDs. Due to the increase of the particle size at higher temperatures, the light harvesting range becomes broader. As a result the band gap decreases from 2 eV at 100 °C to 1.53 eV at 180 °C (Fig. S3b). Among the AZ0–AZ6 QDs synthesized at 180 °C, AZ5 shows the maximum photoluminescence (PL) intensity (Fig. 2c). With higher incorporation of Zn2+ ions, the peak position is slightly blue shifted from AZ0 to AZ6 QDs.28 The room temperature emission spectra of AZ5 QDs were also recorded by taking the aliquots at different reaction temperatures (Fig. 2d). Two distinct emission bands are observed with QDs from aliquots at 100 and 110 °C. The band at higher wavelengths can be attributed to the emission from cation vacancy defects, since at 100–110 °C, Zn2+ ions have minimum probability to enter the vacant sites. The emission band at lower wavelengths arises from donor–acceptor pair recombination within the band gap with Ag+ vacancies as the acceptor, and Se2− and In3+ vacancies as donors (Fig. 2d).29 The intensity of the lower wavelength band gradually increases with an increase in the reaction temperature which indicates higher incorporation of Zn2+ and In3+ into the vacant sites of Ag2Se.14,28,30 At elevated temperatures, these two bands merge into a broad intense emission band. This broad emission band (full width at half maxima >100 nm) is an indication of the formation of alloyed QDs.30 The peak maximum is gradually red shifted due to the faster growth of QDs at higher temperatures. The reaction temperature dependent PL spectra of AZ4 and AZ6 QDs (Fig. S4) show a similar trend to that of AZ5.
image file: c7ta00268h-f2.tif
Fig. 2 (a) Absorption spectra of the colloidal QDs synthesized at 180 °C. (b) Reaction temperature dependent absorption spectra of AZ5 QDs. (c) Relative PL intensity plot of the QDs. (d) Reaction temperature dependent PL spectra of AZ5 QDs. Excitation wavelength: λex = 450 nm. (e) PL lifetime decay plots of colloidal QDs. All spectra were recorded in chloroform. (f) Schematic energy level diagram (not to scale) showing the recombination pathways.

Fig. 2e shows the fluorescence decay curves of all the QDs at an excitation wavelength of 402 nm. The PL decay was recorded at 840, 834, 832 and 830 nm for AZ0, AZ4, AZ5 and AZ6 QDs, respectively. The PL decay profiles are found to be tri-exponential with an average lifetime of 232.7, 180.1, 184.8 and 203.9 ns for AZ0, AZ4, AZ5 and AZ6 QDs, respectively (Table 1). Fig. 2f provides the schematic energy level diagram showing the three recombination pathways with different lifetimes (τ) and their amplitude (A). The faster decay component (τ3 ∼ 2 ns) arises due to non-radiative processes e.g. Auger recombination and its contribution (A3) is the highest in AZ0. In AZ4 to AZ6, the contribution of this component is dominated by surface trap state emission (τ1 ∼ 66.6–75.6 ns) and donor–acceptor recombination (τ3 ∼ 196.4–222.1 ns) between the Ag+ vacancies as donor sites and In3+ and Se2− vacancies as acceptor sites.31 In the absence of Zn2+ (AZ0) the contributions from surface trap state emission and donor–acceptor recombination to the total average lifetime are lower as compared to those of AZ4–AZ6. Since τ2 increases from 196.4 ns to 222.1 ns for AZ4 to AZ6 QDs, respectively, it is evident that Zn2+ diffusion in the In3+ and Ag+ sites allows lesser donor–acceptor recombination. However, the contribution of surface trap state emission (A1) increases from 12.7 for AZ0 to 29.1–30.7 for AZ4–AZ6. The variation of τ1 and A1 implies that Zn2+ ions occupy surface sites till saturation before diffusing to the vacancy sites inside the AgInSe2 lattice. This is manifested from similar band gaps of AZ0 and AZ4, before increasing for AZ5 and AZ6 by Zn2+ lattice diffusion. In this case, segregation of a separate ZnSe phase at the QD surface is possible; however no such evidence is obtained from the XRD patterns in Fig. 1a.

Table 1 PL lifetime decay parameters of QDs synthesized at 180 °C
QD code A 1 τ 1 (ns) A 2 τ 2 (ns) A 3 τ 3 (ns) χ 2 τ〉 (ns)
AZ0 12.68 37.7 53.15 240.8 34.17 1.33 1.13 232.7
AZ4 29.49 66.6 69.65 196.4 0.85 2.67 1.04 180.1
AZ5 30.68 67.9 68.23 202.5 1.09 1.69 1.09 184.8
AZ6 29.08 75.6 70.07 222.1 0.85 1.94 1.06 203.9


2.2 Photovoltaic performance of the QDs

The working electrodes were prepared by dip coating of the as-prepared ∼9 μm thick TiO2 films on fluorine-doped tin oxide (FTO) coated glass substrates in aqueous dispersions of MPA-capped QDs. With the counter electrode made of a paste of microwave synthesized CuS powder32 and the sandwiched droplet of the electrolyte between the working and counter electrodes, at first the performance of AZ0–AZ6 based QDSSCs was tested. Here 8 cycles of ZnS passivation layers were applied on the working electrode by successive ionic layer adsorption and reaction (SILAR). Second, the number of ZnS SILAR cycles was optimized with the best performing QDs. In the third step, a double inorganic passivation of amorphous TiO2 and SiO2 was applied to further enhance the photovoltaic performance. Electrochemical impedance spectroscopy (EIS) was used to explain the trends and the role of passivation.
2.2.1 Performance of AISE and ZAISE QDSSCs. The current density (J)–voltage (V) characteristics of the QDSSCs fabricated with AZ0–AZ6 QDs are shown in Fig. 3a. The open circuit voltage (VOC), JSC, fill factor (FF) and PCE (η%) of the QDSSCs are tabulated in Table 2 where 8 ZnS SILAR cycles were applied in all the QDSSCs. The variation of all the solar cell parameters is shown in Fig. 3b and c as a function of Zn/(Ag + In) at%. VOC increases from 0.30 V for AZ0 to 0.37 V for AZ5 films and decreases for AZ6. The photocurrent also shows a similar trend where the highest JSC is observed for AZ5 (15.78 mA cm−2) as compared to AZ0 (9.91 mA cm−2). The photovoltaic performance was observed to be the highest for AZ5 QDSSCs (3.07%) which is 45.6% more than that of AZ0 QDSSCs (1.67%).
image file: c7ta00268h-f3.tif
Fig. 3 (a) JV characteristics of the QDSSCs under 1 sun illumination. (Inset) Digital images of AZ0 and AZ5 photoanodes. Variation of the (b) JSC and VOC, and (c) PCE of the QDSSCs as a function of Zn/(Ag + In) at%. (d) Nyquist plot of the QDSSCs at −0.35 V forward bias under dark conditions with the equivalent circuit as the inset. Plots of the (e) recombination resistance and (f) chemical capacitance of the QDSSCs with applied potential. (g) Variation of dark current with applied potential in the log scale (inset shows the normal scale).
Table 2 QDSSC parameters after treatment of 8 ZnS cycles by SILAR
QDSSCs Zn/(Ag + In) at% J SC (mA cm−2) V OC (V) FF η (%)
a Average of three cells in parallel.
AZ0 0 9.91 ± 0.54 0.302 ± 0.004 0.555 ± 0.006 1.67 ± 0.10
AZ4 36.2 13.13 ± 0.16 0.320 ± 0.004 0.526 ± 0.013 2.24 ± 0.07
AZ5 48.2 15.78 ± 0.19 0.368 ± 0.011 0.529 ± 0.013 3.07 ± 0.02
AZ6 57.9 12.87 ± 0.13 0.308 ± 0.004 0.520 ± 0.007 2.07 ± 0.01


The EIS measurements were carried out in the dark to highlight the significant improvement of the device efficiency upon zinc incorporation into the QDs.33Fig. 3d shows the Nyquist plots recorded in the frequency range from 0.1 Hz to 1 MHz at a forward bias of −0.35 V, which is very close to the VOC of the QDSSCs. The Nyquist plots are fitted with an equivalent circuit as shown in the Fig. 3d inset. All the EIS parameters e.g. series resistance (Rs), charge recombination resistance at photoanode and electrolyte interfaces (Rrec), and chemical capacitance (Cμ) are tabulated in Table 3. No significant change of Rs is observed for different QDSSCs since it depends upon the transport resistance of FTO and the connection setup which is equivalent for all the measurements. However, a considerably higher Rrec is observed in ZAISE than AISE QDSSCs (Fig. 3e). Since Rrec is inversely proportional to the charge recombination rate, the latter becomes sluggish at the interface of the ZAISE photoanode and the electrolyte than with the AISE photoanode. The photovoltaic data shown in Table 2 can be directly correlated with Rrec data which shows the significant improvement of the efficiency of ZAISE based devices. The Cμ of all the QDSSCs is similar at different applied voltages (Fig. 3f), due to the unchanged TiO2 conduction band position with different QD sensitizers. As a cross-check on the recombination rate in QDSSCs, their IV characteristics were also measured in the dark (Fig. 3g inset) and the dark or recombination current is plotted as a function of applied voltage (Fig. 3g). The dark current in ZAISE QDSSCs is less than that in AISE QDSSCs at the same applied voltage which further proves the slower charge recombination at the photoanode/electrolyte interfaces in ZAISE QDSSCs.

Table 3 EIS parameters of QDSSCs after different post treatment processes
QDSSCSs R s (Ω cm−2) R rec (Ω cm−2) C μ (mF cm−2) f max (Hz) τ n (ms)
AZ0-8Z 10.65 12.58 0.70 12.12 13.11
AZ4-8Z 15.34 17.06 0.64 8.25 19.26
AZ5-8Z 12.25 30.78 0.68 5.62 28.27
AZ6-8Z 11.88 15.98 0.62 10.00 15.90
AZ5-4Z 12.1 21.58 0.67 8.25 19.26
AZ5-10Z 14.8 27.61 0.63 6.81 23.34
AZ5-8ZTS 12.75 46.87 0.65 3.83 41.50


The relatively higher efficiency of AZ5 QDSSCs even though the average lifetime of AZ5 colloidal QDs is lower than those of AZ0 and AZ6 is quite intriguing (Table 1). When the QD surface layer is passivated by 8 ZnS SILAR cycles, the surface trap state recombination is reduced. Since AZ5 has a relatively higher contribution of τ1, the QDSSCs with AZ5 QDs are mostly benefitted. Interestingly in this work, a total of 8 ZnS SILAR cycles are required to make a well passivated layer on the QD surface whereas there are reports where 4 ZnS SILAR cycles are employed to achieve the highest device efficiency.2,34,35 This clearly highlights the importance of reducing the surface trap state emission. The surface passivation however cannot alter the τ2 and τ3 components i.e. non-radiative and donor–acceptor recombination processes which are inherent to the QDs with a specific Zn2+ concentration. Due to the reduction in surface trap states, slower charge recombination occurs at the TiO2/QD/electrolyte interface which increases the PCE of AZ5-8Z QDSSCs. On the other hand, due to a large amount of non-radiative loss, PCE is the least for AZ0-8Z QDSSCs (Table 2).

2.2.2 Variation of ZnS SILAR cycles. To probe the extent of passivation, the number of the ZnS SILAR cycles was varied and applied onto the AZ5-fabricated QDSSCs. The cells are denoted as AZ5-4Z, AZ5-8Z and AZ5-10Z for 4, 8 and 10 ZnS SILAR cycles, respectively. The photocurrent increases by 31.2% from AZ5-4Z to AZ5-8Z (Table S1) due to surface passivation of unsaturated dangling bonds and surface trap states of the QDs. VOC also increases from 0.34 V for AZ5-4Z to 0.37 V for AZ5-8Z whereas FF also shows a similar trend. From AZ5-8Z to AZ5-10Z, although JSC and FF remain almost constant, VOC decreases. Thus, the overall PCE is the highest with 8 ZnS cycles (Fig. S5). Rrec is significantly higher for AZ5-8Z and AZ5-10Z compared to AZ5-4Z. However Cμ is lower for AZ5-10Z at different applied voltages, a trend similar to an earlier report for CuInSe2 QDSSCs with a higher number of ZnS cycles.36 The deposition of passivation layers beyond the optimum thickness can partially block the TiO2 pores leading to poor infiltration of the electrolyte.2 10 ZnS SILAR cycles can agglomerate the QDs which limits the interfacial contact between porous TiO2 and the polysulfide electrolyte and therefore with a limiting charge injection propensity, PCE does not improve beyond that of AZ5-8Z. The blocking of pores may promote processes such as auger recombination or radiative recombination due to the presence of long lived holes in the ZAISE QDs and limited hole transfer from QDs to the electrolyte.35
2.2.3 Effect of TiO2/SiO2 double passivation. With the goal to improve the PCE beyond 3.07%, the photoanode containing 8 ZnS SILAR cycles was enriched with amorphous TiO2 and SiO2 passivation layers to make AZ5-8ZTS cells. These double passivation layers increase both JSC and VOC as shown in Fig. 4a and tabulated in Table 4. A very significant change in FF is observed from 0.53 for AZ5-8Z to 0.59 for AZ5-8ZTS. By following these techniques, the best PCE of 3.57% is achieved for AZ5-8ZTS QDSSCs which is 15.9% higher than that of AZ5-8Z QDSSC. Likewise the charge recombination is also reduced as shown in Fig. 4b and c. Although Rrec does not improve from 8 to 10 ZnS cycles, a very thin SiO2 layer on top of 8 cycles of ZnS can slow down the recombination rate by saturating the dangling bonds through Ti–S and Zn–O bond formation without any change in Cμ (Fig. 4d). The lifetime of the electrons (τn) is calculated from the Bode plot (Fig. 4e) by using eqn (1):
 
τn = 1/(2πfmax)(1)
where fmax is the frequency maxima of the lower frequency peak in the Bode plot. The calculated lifetime of AZ0-8Z, AZ5-8Z and AZ5-8ZST QDSSCs is 13.1, 28.3 and 41.5 ms, respectively (Table 3). This higher recombination lifetime of the electrons further confirms the slower charge recombination processes after applying amorphous TiO2 on top of the QD layer and SiO2 on the ZnS layer. This result is further supported by the dark current measurements at different applied voltages (Fig. 4f).

image file: c7ta00268h-f4.tif
Fig. 4 (a) JV characteristics of the representative QDSSCs under 1 sun illumination. (Inset) Digital image of the AZ5-8ZTS photoanode. (b) Nyquist plot of the QDSSCs at −0.35 V forward bias under dark conditions. Plots of the (c) recombination resistance and (d) chemical capacitance of the QDSSCs with applied potential. (e) Bode plots of the QDSSCs. (f) Variation of dark current with applied potential in the log scale.
Table 4 QDSSC parameters for AZ0 and AZ5 after different post treatments
QDSSCs J SC (mA cm−2) V OC (V) FF η (%)
a Average of three cells in parallel. b Champion cell.
AZ0-8Z 9.91 ± 0.54 0.302 ± 0.004 0.555 ± 0.006 1.67 ± 0.10
AZ5-8Z 15.78 ± 0.19 0.368 ± 0.011 0.529 ± 0.013 3.07 ± 0.02
AZ5-8ZTSa 15.78 ± 0.23 0.378 ± 0.002 0.576 ± 0.016 3.41 ± 0.16
AZ5-8ZTSb 16.03 0.381 0.585 3.57


Several charge recombination processes which are responsible for the low PCE of QDSSCs include band edge recombination between the valence band holes and the conduction band electrons in QDs, back electron transfer to the electrolyte from photoexcited electrons of QDs and from the conduction band of TiO2, recombination of conduction band electrons of TiO2 with the valence band hole of QDs, and surface trapping of photoexcited electrons of QDs and conduction band electrons of TiO2.37 The modification of the photoanode surface with suitable inorganic and organic passivation layers is a key step to suppress these charge recombination pathways and improve the device efficiency.38–40 Inorganic passivation can suppress a majority of these recombination pathways which indeed is the key step to enhance the PCE of QDSSCs.34,41,42 In this work, when ZnS is deposited by SILAR onto the QD-coated TiO2 substrate, it likely passivates the dangling bonds present on the TiO2 surface through the formation of well-ordered Zn–O and S–Ti bonds. The amorphous TiO2 coating, on the QD-deposited TiO2 photoanode, acts as a buffer layer at the interface between TiO2/QDs and ZnS/SiO2 thus reducing the interfacial trap states to enhance the device efficiency. Further, the deposition of SiO2 on ZnS can passivate all the exposed Zn and S surface atoms through the formation of Si–S and O–Zn bonds at the interface of ZnS and SiO2.35 The coating of these different inorganic passivation layers is evident in the TEM image of the photoanode (Fig. S6). However, the separate layers could not be distinguished in the ∼1.5 nm thick amorphous coating. The energy dispersive analysis of X-rays (EDAX) and elemental mapping in fact confirm the presence of Zn, S, O and Si elements.

To understand the role of passivation layers, QDs were deposited onto an insulating mesoporous SiO2 layer on FTO glass. Since there will be no charge injection from the QDs into the SiO2 layer, the changes in PL spectra (Fig. S7) with different passivation layers can verify the significance of passivation. The PL intensity decreases by coating of an amorphous TiO2 layer onto the QDs due to injection of charge from QDs into TiO2. The PL intensity increases again by applying ZnS and SiO2 coatings over the film due to surface passivation of the QDs. ZnS and TiO2/SiO2 passivation however will be able to control neither the band edge recombination in QDs, nor the recombination pathways between QDs and the TiO2 photoanode which remain in contact without any interfacial layer. In fact these passivation layers at the interface of the photoanode and electrolyte potentially reduce or stop the back electron transfer from photoexcited electrons of QDs and from the conduction band of TiO2 to the electrolyte. A schematic is shown in Fig. 5 where the desired electron transfer pathways are shown by thicker curved arrows and the undesired recombination pathways are shown with dotted arrows. Overall, this strategic combination of alloying with Zn in AISE QDs, optimized ZnS layers and TiO2/SiO2 double passivation could significantly enhance the PCE of AISE based QDSSCs to 3.57%, which is ∼23% higher than the best of previous reports (Table 5).10,15–18,22,43–45


image file: c7ta00268h-f5.tif
Fig. 5 Schematic of the AZ5-8ZTS based QDSSC showing the electron transfer (solid curved arrows) and recombination pathways (dotted straight arrows).
Table 5 Review of literature reports on AgInS2/Se2 solar cells
QD Synthesis method Deposition methodb Nature of devices PCE (%) Ref.
a HI = hot-injection method; HU = heating-up method. b SA = self-assembly; EPD = electrophoretic deposition; NA = not available.
Cu diffused AgInS2 HI + HUa Spin coating Bulk heterojunction 1.13 22
ZnO/ZnS/AgInS2 nanotube arrays NA Chemical etching + anion exchange + autoclave Inorganic–organic hybrid solar cell 2.11 18
AgInS2 Ligand-free synthesis Direct deposition Liquid junction 0.80 10
ZnSe-AgInSe2/CdS HU SA + SILARb Liquid junction 1.90 43
Ag2S/AgInS2 heterostructures HI NA Bulk heterojunction 0.52 15
Ag2S/AgInS2 nanoheterodimers Thermolysis Direct deposition Liquid junction 1.30 16
AgInS2/In2S3 NA SILAR Liquid junction 0.70 17
AgInS2-ZnS HI EPD Liquid junction 2.25 44
AgInS2 HU SA via ligand exchange Liquid junction 2.9 45
Zn-AgInSe2 HI + HU SA via ligand exchange Liquid junction 3.57 This work


3. Conclusions

Zn2+-diffused AgInSe2 QDs with a Zn:(Ag + In) at% of 36, 48 and 58 were synthesized by a hot-injection method and applied as light harvesters in QDSSCs. A majority of Zn2+ ions occupy the In3+ sites over Ag+ sites. The QDs had a broad light harvesting range from the visible to the NIR region and the PL lifetime decreases with Zn2+-diffusion up to a Zn:(Ag + In) at% of 48.2 (AZ5). The AISE and ZAISE QDs were ligand-exchanged with MPA to achieve a maximum loading of the QDs on the TiO2 photoanode. Apart from improving the crystallinity and carrier mobility of the QDs, diffusion of Zn2+ also tunes the intrinsic band gap. With 8 SILAR cycles of ZnS on top of the QD-deposited TiO2 photoanode the PCE was improved from 1.67% for AZ0 to 3.07% for AZ5. The passivation by ZnS reduces the surface trap state recombination whereas the non-radiative and donor–acceptor recombination processes likely remain unchanged. The PCE was further enhanced to 3.57% by dual inorganic passivation according to the TiO2/QD/amorphous TiO2/ZnS/SiO2 configuration. In addition to the suppression of surface trap states, the surface passivation reduces the recombination pathways of back electron transfer from photoexcited electrons of QDs and also from the conduction band of TiO2 to the polysulfide redox electrolyte. The record PCE of 3.57% is so far the highest achieved for ternary AgInX2 (X = S, Se) based QDSSCs. A similar strategy coupled with a surface passivation approach is effective in enhancing the device efficiency of other low performing QD systems in photovoltaic applications.

4. Experimental section

4.1 Materials

Silver nitrate (AgNO3, Sigma Aldrich, 98%), indium chloride tetrahydrate (InCl3·4H2O, Sigma Aldrich, 99.999%), oleylamine (Sigma Aldrich, ≥98%), 1-octadecene (Sigma Aldrich, technical grade, 90%), 1-dodecanethiol (Sigma Aldrich, ≥98%), zinc acetate dihydrate Zn(OAc)2·2H2O (Merck India, 98%), zinc nitrate hexahydrate Zn(NO3)2·6H2O (reagent grade, 98%), sulfur powder (purified, Merck India), sodium sulfide flakes (Na2S·9H2O, purified, Merck India), potassium chloride (purified, Merck India), chloroform (Emplura, Merck India), ethanol (Absolute, Changshu Yangyuan, China) and methanol (Sigma Aldrich, ACS spectrophotometric grade, 98%) were used without further purification.

4.2 Synthesis methodologies

The synthesis of AISE QDs was performed by following a literature reported method with slight modifications.30
4.2.1 Preparation of selenium stock solution. 1 mmol Se powder, 1 mL oleylamine and 1 mL dodecane thiol were taken in a round bottomed flask followed by evacuation and refilling with N2 three times at room temperature. Then the mixture was stirred under N2 to dissolve the Se powder.
4.2.2 Synthesis of AISE QDs. In a separate three neck round bottomed flask, 0.5 mmol AgNO3, 0.5 mmol InCl3·4H2O, 12 mL octadecene and 6 mL of oleylamine were loaded and cycled between vacuum and N2 three times at 60 °C. Then, the mixture was heated to 88 °C. When the target temperature was achieved, 2 mL of Se stock solution was rapidly injected into it. The solution immediately turned dark brown. The mixture was again heated to 180 °C for QD-growth and aged at this temperature for 5 min. Finally, the reaction was quenched in a water bath and the product was isolated by precipitation with ethanol followed by centrifugation at 6500 rpm. The QDs were redispersed in chloroform for further use.
4.2.3 Synthesis of ZAISE QDs. 0.5 mmol AgNO3, 0.5 mmol InCl3·4H2O and Zn(OAC)2·2H2O (varied from 0.02 to 0.06 mmol) were loaded into a three-neck round bottomed flask along with 6 mL of oleylamine and 12 mL of octadecene. The reaction mixture was cycled between vacuum and N2 three times at 60 °C. Then, the mixture was heated to 88 °C. When the temperature reached 85 °C, the transparent colorless solution turned milky white. Then, 2 mL of Se-precursor solution was quickly injected into the above mentioned solution at 88 °C. The solution immediately turned dark brown and the mixture was further heated to 180 °C and kept at this temperature for 5 min. Finally, the reaction mixture was quenched in a water bath and the mixture was precipitated with ethanol followed by centrifugation. Finally the ZAISE QDs were redispersed in CHCl3 and stored in the dark for further use.
4.2.4 Preparation of water soluble MPA-capped AISE and ZAISE QDs. The water soluble AISE and ZAISE QDs were prepared by replacing the initial hydrophobic oleylamine group with MPA. At first, 500 μL MPA was taken into a vial along with 4 mL MeOH and 1 mL distilled water. The pH of this solution was adjusted to 12 with 5 M NaOH. 0.5 mmol of AISE QDs dispersed into chloroform was taken into a separate vial and MPA-methanol solution was added to it followed by stirring for 4 h. Post stirring, the mixture was allowed to stand for few minutes to separate the phases. The bottom organic layer was discarded. The upper aqueous layer containing the QDs was washed with acetone to remove free MPA molecules and QDs were redispersed in 6 mL water for further use.
4.2.5 Synthesis of CuxS nanostructures. CuxS nanostructures were synthesized by following our previously reported method.32 5 mmol Cu(NO3)2·6H2O and 5 mmol sulfur powder in 100 mL ethylene glycol were taken in a round bottomed flask and irradiated in a microwave chamber at 125 °C for 12 min at 600 W. The color of the solution changed from blue to deep green and a black colored product was precipitated. Finally, the product was washed with ethanol by centrifugation at 5000 rpm for 5 min and dried at 80 °C for 1 h to obtain the CuxS nanostructures.

4.3 Fabrication of QDSSCs

4.3.1 Preparation of the TiO2 photoanode. FTO coated glass (Solaronix, TCO 22-7, 2.2 mm thickness) pieces were cleaned ultrasonically with soap water followed by distilled water and ethanol. Three different layers of TiO2 were sequentially deposited onto the FTO glasses. At first, a compact layer was deposited by immersing the cleaned glasses into an aqueous solution of 40 mM TiCl4 at 80 °C for 45 min followed by washing with distilled water and ethanol. Active and scattering layers were deposited by the doctor blade technique. The active layer was prepared on top of the compact layer by using a TiO2 paste (Solaronix, Ti-Nanoxide T/SP, particle size ∼20 nm) followed by annealing at 500 °C in air for 1 h in a furnace (film thickness ∼10 μm). A ∼4 μm thick scattering layer of TiO2 (Solaronix, Ti-Nanoxide R/SP, particle size ∼100 nm) was then coated on the active layer followed by annealing at 500 °C for another 1 h.
4.3.2 Sensitization of the TiO2 photoanode. MPA-capped QDs were dispersed into 6 mL deionized water. 53 μL of MPA was added to the dispersion and the pH was maintained at 12 with 5 M NaOH. The TiO2 films were dipped into this solution for sensitization and kept for 24 h. Finally, the QD sensitized TiO2 films were washed with distilled water and kept for further use.
4.3.3 Preparation of the ZnS passivation layer. To passivate the QD layer, a very thin layer of ZnS was employed onto the QD deposited TiO2 films by SILAR. At first, the QD-deposited TiO2 photoanode was dipped into an aqueous solution of 0.1 M Zn(NO3)2·6H2O solution for 1 min followed by rinsing with distilled water. The electrodes were further dipped into 0.1 M Na2S·9H2O solution for another 1 min. The electrodes were further rinsed with distilled water to remove the unbound S2− ions. The protocol was repeated to achieve the desired number of SILAR cycles.
4.3.4 Preparation of TiO2 and SiO2 double passivation layers. Amorphous TiO2 and SiO2 double passivation layers were prepared by following the literature reported method.34,35 At first, the QDSSCs before ZnS treatment were dipped into 10 mM aqueous solution of TiCl4 and kept at 40 °C for 30 min to create a very thin layer of amorphous TiO2 over the QD deposited TiO2 photoanode. Then the films were washed with distilled water followed by ethanol. Thereafter the ZnS passivation layer was applied as per the above protocol followed by rinsing with distilled water. These films were further immersed into an ethanolic solution of tetraethyl orthosilicate and kept for 2 h. Finally the electrodes were washed with ethanol for further use.
4.3.5 Preparation of the CuxS counter electrode. A paste of CuxS was prepared by stirring overnight a mixture of CuxS nanostructures and polyvinyledene fluoride (10[thin space (1/6-em)]:[thin space (1/6-em)]1 w/w) in N-methyl 2-pyrrolidone. The paste was doctor bladed on pre-cleaned FTO, dried and annealed at 80 °C for 1.5 h.
4.3.6 Electrolyte. A mixture of 2 M Na2S, 2 M S and 0.2 M KCl solutions in methanol/H2O (3[thin space (1/6-em)]:[thin space (1/6-em)]7 v/v) was employed as the electrolyte.
4.3.7 Preparation of QDSSCs. The QDSSCs were prepared by assembling the counter electrode and the QD-sensitized photoanode using a 50 μm thick parafilm spacer in a sandwich configuration. A 50 μL droplet of the polysulfide electrolyte was employed between the two electrodes before assembling them. The active area was selected by employing a mask onto the working electrodes. The active area of the electrode was 0.23 cm2.

4.4 Characterization

The XRD measurements were carried out with a Rigaku powder X-ray diffractometer having Cu Kα = 1.54059 Å radiation. The ICP-MS measurements were performed by using a Thermo Scientific X-series using Plasma lab software. TEM images were obtained with a UHR-FEG TEM system (JEOL, Model JEM 2100 F) using a 200 kV electron source equipped with an energy dispersive X-ray spectroscope. To record the TEM images, EDAX and elemental mapping, the QD-sensitized photoanode with different inorganic coatings was crushed to powder and dispersed in isopropanol. UV-Vis absorbance spectra of the QD dispersion and the TiO2 photoanode were recorded using a Jasco V-670 spectrophotometer. To record the absorbance spectra of the TiO2 photoanode, the spectrophotometer was equipped with an integrating sphere. Room temperature PL spectra were measured with a Horiba Jobin Yvon Fluorolog using a Xe lamp as the excitation source with an excitation wavelength of 480 nm. The fluorescence lifetimes were recorded by using a time correlated single-photon counting spectrofluorimeter from HORIBA Jobin Yvon IBH. The fluorescence life time was calculated by fitting the decay curves by using an iterative fitting program provided by IBH. Photovoltaic measurements were carried out by using a solar simulator provided by Newport using a 300 W xenon lamp as a light source. The intensity of the light was adjusted to 100 mW cm−2 by using a reference silicon solar cell in the presence of a 1.5 G filter. The photovoltaic and the impedance measurements were carried out by using a CHI Electrochemical workstation. The plots were analyzed with inbuilt software in the electrochemical workstation.

Acknowledgements

GH thanks the University Grants Commission (UGC), New Delhi for her fellowship. GH also thanks Dr M. Venkataramanan for his help with the PL measurements and Mr Arjun Halder for the XRD measurements. The financial support from the Department of Science & Technology – Science & Engineering Research Board (DST-SERB) under Sanction No EMR/2016/001703 is duly acknowledged. SB thanks IISER Kolkata for the academic and research fund.

Notes and references

  1. M. C. Beard, J. Phys. Chem. Lett., 2011, 2, 1282–1288 CrossRef CAS PubMed .
  2. A. Sahasrabudhe and S. Bhattacharyya, Chem. Mater., 2015, 27, 4848–4859 CrossRef CAS .
  3. O. E. Semonin, J. M. Luther, S. Choi, H.-Y. Chen, J. Gao, A. J. Nozik and M. C. Beard, Science, 2011, 334, 1530–1533 CrossRef CAS PubMed .
  4. A. J. Nozik, Chem. Phys. Lett., 2008, 457, 3–11 CrossRef CAS .
  5. P. V. Kamat, Acc. Chem. Res., 2012, 45, 1906–1915 CrossRef CAS PubMed .
  6. P. V. Kamat, J. Phys. Chem. C, 2007, 111, 2834–2860 CAS .
  7. Z. Pan, K. Zhao, J. Wang, H. Zhang, Y. Feng and X. Zhong, ACS Nano, 2013, 7, 5215–5222 CrossRef CAS PubMed .
  8. Z. Pan, I. Mora-Seró, Q. Shen, H. Zhang, Y. Li, K. Zhao, J. Wang, X. Zhong and J. Bisquert, J. Am. Chem. Soc., 2014, 136, 9203–9210 CrossRef CAS PubMed .
  9. W. Li, Z. Pan and X. Zhong, J. Mater. Chem. A, 2015, 3, 1649–1655 CAS .
  10. K. P. Kadlag, P. Patil, M. J. Rao, S. Datta and A. Nag, CrystEngComm, 2014, 16, 3605–3612 RSC .
  11. M. G. Panthani, C. J. Stolle, D. K. Reid, D. J. Rhee, T. B. Harvey, V. A. Akhavan, Y. Yu and B. A. Korgel, J. Phys. Chem. Lett., 2013, 4, 2030–2034 CrossRef CAS PubMed .
  12. G. Halder and S. Bhattacharyya, J. Phys. Chem. C, 2015, 119, 13404–13412 CAS .
  13. J. Krustok, J. Raudoja, M. Krunks, H. Mändar and H. Collan, J. Appl. Phys., 2000, 88, 205–209 CrossRef CAS .
  14. B. Mao, C.-H. Chuang, F. Lu, L. Sang, J. Zhu and C. Burda, J. Phys. Chem. C, 2013, 117, 648–656 CAS .
  15. R. Bose, G. Manna, S. Jana and N. Pradhan, Chem. Commun., 2014, 50, 3074–3077 RSC .
  16. M. Jagadeeswararao, A. Swarnkar, G. B. Markad and A. Nag, J. Phys. Chem. C, 2016, 120, 19461–19469 CAS .
  17. Y. Wang, Q. Zhang, Y. Li and H. Wang, Nanoscale, 2015, 7, 6185–6192 RSC .
  18. J. Han, Z. Liu, K. Guo, J. Ya, Y. Zhao, X. Zhang, T. Hong and J. Liu, ACS Appl. Mater. Interfaces, 2014, 6, 17119–17125 CAS .
  19. D. Aldakov, A. Lefrançois and P. Reiss, J. Mater. Chem. C, 2013, 1, 3756–3776 RSC .
  20. G. Hodes, J. Phys. Chem. C, 2008, 112, 17778–17787 CAS .
  21. H. McDaniel, N. Fuke, N. S. Makarov, J. M. Pietryga and V. I. Klimov, Nat. Commun., 2013, 4, 2887 Search PubMed .
  22. A. Guchhait and A. J. Pal, ACS Appl. Mater. Interfaces, 2013, 5, 4181–4189 CAS .
  23. A. G. Pattantyus-Abraham, I. J. Kramer, A. R. Barkhouse, X. Wang, G. Konstantatos, R. Debnath, L. Levina, I. Raabe, M. K. Nazeeruddin, M. Grätzel and E. H. Sargent, ACS Nano, 2010, 4, 3374–3380 CrossRef CAS PubMed .
  24. J. Du, Z. Du, J.-S. Hu, Z. Pan, Q. Shen, J. Sun, D. Long, H. Dong, L. Sun, X. Zhong and L.-J. Wan, J. Am. Chem. Soc., 2016, 138, 4201–4209 CrossRef CAS PubMed .
  25. M. A. Ahmed, K. E.-S. Rady, K. M. El-Shokrofy, A. A. Arais and M. S. Shams, Mater. Sci. Appl., 2014, 5, 932–942 CAS .
  26. J. E. Jaffe and A. Zunger, Phys. Rev. B: Condens. Matter, 1984, 29, 1882 CrossRef CAS .
  27. A. R. Kirmani, A. Kiani, M. M. Said, O. Voznyy, N. Wehbe, G. Walters, S. Barlow, E. H. Sargent, S. R. Marder and A. Amassian, ACS Energy Lett., 2016, 1, 922–930 CrossRef CAS .
  28. X. Tang, W. B. A. Ho and J. M. Xue, J. Phys. Chem. C, 2012, 116, 9769–9773 CAS .
  29. B. Chen, H. Zhong, W. Zhang, Z. Tan, Y. Li, C. Yu, T. Zhai, Y. Bando, S. Yang and B. Zou, Adv. Funct. Mater., 2012, 22, 2081–2088 CrossRef CAS .
  30. D. Yao, H. Liu, Y. Liu, C. Dong, K. Zhang, Y. Sheng, J. Cui, H. Zhang and B. Yang, Nanoscale, 2015, 7, 18570–18578 RSC .
  31. B. Mao, C.-H. Chuang, J. Wang and C. Burda, J. Phys. Chem. C, 2011, 115, 8945–8954 CAS .
  32. D. Ghosh, G. Halder, A. Sahasrabudhe and S. Bhattacharyya, Nanoscale, 2016, 8, 10632–10641 RSC .
  33. A. Sahasrabudhe, S. Kapri and S. Bhattacharyya, Carbon, 2016, 107, 395–404 CrossRef CAS .
  34. Z. Ren, J. Wang, Z. Pan, K. Zhao, H. Zhang, Y. Li, Y. Zhao, I. Mora-Sero, J. Bisquert and X. Zhong, Chem. Mater., 2015, 27, 8398–8405 CrossRef CAS .
  35. K. Zhao, Z. Pan, I. Mora-Seró, E. Cánovas, H. Wang, Y. Song, X. Gong, J. Wang, M. Bonn, J. Bisquert and X. Zhong, J. Am. Chem. Soc., 2015, 137, 5602–5609 CrossRef CAS PubMed .
  36. J.-Y. Kim, J. Yang, J. H. Yu, W. Baek, C.-H. Lee, H. J. Son, T. Hyeon and M. J. Ko, ACS Nano, 2015, 9, 11286–11295 CrossRef CAS PubMed .
  37. J. Tian and G. Cao, J. Phys. Chem. Lett., 2015, 6, 1859–1869 CrossRef CAS PubMed .
  38. K. Zhao, Z. Pan and X. Zhong, J. Phys. Chem. Lett., 2016, 7, 406–417 CrossRef CAS PubMed .
  39. N. Guijarro, J. M. Campiña, Q. Shen, T. Toyoda, T. Lana-Villarreal and R. Gómez, Phys. Chem. Chem. Phys., 2011, 13, 12024–12032 RSC .
  40. Z. Liu, M. Miyauchi, Y. Uemura, Y. Cui, K. Hara, Z. Zhao, K. Sunahara and A. Furube, Appl. Phys. Lett., 2010, 96, 233107 CrossRef .
  41. Z. Ren, Z. Wang, R. Wang, Z. Pan, X. Gong and X. Zhong, Chem. Mater., 2016, 28, 2323–2330 CrossRef CAS .
  42. Z. Pan and X. Zhong, J. Mater. Chem. A, 2016, 4, 18976–18982 CAS .
  43. T. Kameyama, Y. Douke, H. Shibakawa, M. Kawaraya, H. Segawa, S. Kuwabata and T. Torimoto, J. Phys. Chem. C, 2014, 118, 29517–29524 CAS .
  44. S. M. Kobosko, D. H. Jara and P. V. Kamat, ACS Appl. Mater. Interfaces DOI:10.1021/acsami.6b14604 .
  45. C. Cai, L. Zhai, Y. Ma, C. Zou, L. Zhang, Y. Yang and S. Huang, J. Power Sources, 2017, 341, 11–18 CrossRef CAS .

Footnote

Electronic supplementary information (ESI) available: Powder XRD pattern of Ag2Se; Tauc plots; PL spectra of AZ4 and AZ6 QDs synthesized at different temperatures; JV characteristics and variation of Nyquist plots, Rrec and Cμ as a function of the bias voltage of AZ5 QDSSCs with different ZnS SILAR cycles. See DOI: 10.1039/c7ta00268h

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.